{"id":4294,"date":"2026-10-08T15:37:52","date_gmt":"2026-10-08T15:37:52","guid":{"rendered":"https:\/\/www.tgsteels.com\/?page_id=4294"},"modified":"2026-10-12T13:55:16","modified_gmt":"2026-10-12T13:55:16","slug":"1-3247-m42","status":"publish","type":"page","link":"https:\/\/www.tgsteels.com\/cs\/rychlorezne-oceli\/1-3247-m42\/","title":{"rendered":"3247 PRIME"},"content":{"rendered":"[vc_row type=&#8220;full_width_background&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; video_bg=&#8220;use_video&#8220; video_mp4=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.mp4&#8243; video_webm=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.webm&#8220; video_ogv=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.ogv&#8220; background_video_loading=&#8220;default&#8220; scene_position=&#8220;center&#8220; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; parallax_bg=&#8220;true&#8220; parallax_bg_speed=&#8220;fast&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/2&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220; column_padding_type=&#8220;default&#8220; gradient_type=&#8220;default&#8220;][divider line_type=&#8220;No Line&#8220; custom_height=&#8220;450&#8243;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<h1>3247 PRIME <span style=\"display:block;font-size:.5em;line-height:1.35;margin-top:.4em\">(1.3247, HS2-9-1-8, X110MoCoCrWV10-8-4-2-1, W2Mo9Cr4VCo8, SKH59, BM42, M42)<\/span><\/h1>\n[\/vc_column_text][divider line_type=&#8220;No Line&#8220; custom_height=&#8220;50&#8243;][\/vc_column][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/2&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h4>P\u0159etaven\u00e1 rychlo\u0159ezn\u00e1 ocel s vysokou odolnost\u00ed proti opot\u0159eben\u00ed v kombinaci s vysokou tvrdost\u00ed za tepla<\/h4>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<p>3247 PRIME;<\/p>\n<ul>\n<li>je elektrostruskov\u011b p\u0159etaven\u00e1 <em>(ESR)<\/em> rychlo\u0159ezn\u00e1 ocel, velmi vysok\u00e9 \u010distoty a velmi jemn\u00e9 struktury, co\u017e zvy\u0161uje jej\u00ed hou\u017eevnatost.<\/li>\n<li>m\u00e1 vysok\u00fd obsah kobaltu, kter\u00fd j\u00ed dod\u00e1v\u00e1 vysokou tvrdost za tepla a velmi vysokou odolnost proti k\u0159ehnut\u00ed p\u0159i popou\u0161t\u011bn\u00ed.<\/li>\n<li>vyzna\u010duje se vysokou odolnost\u00ed proti opot\u0159eben\u00ed v kombinaci s vysokou tvrdost\u00ed a dobrou hou\u017eevnatost\u00ed.<\/li>\n<li>vlastnostmi vyhovuje povrchov\u00fdm \u00faprav\u00e1m, jako je nitridace v plynov\u00e9, iontov\u00e9 nebo soln\u00e9 l\u00e1zni, a tak\u00e9 pro povlaky PVD nebo CVD.<\/li>\n<\/ul>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Pou\u017eit\u00ed<\/h3>\n<p>3247 PRIME lze pou\u017e\u00edvat na: jemn\u00e9 \u0159ezn\u00e9 n\u00e1stroje <em>(razn\u00edky a matrice)<\/em>, n\u00e1stroje pro tv\u00e1\u0159en\u00ed za studena nebo za tepla <em>(razn\u00edky a matrice)<\/em>.<\/p>\n<p>3247 PRIME je tak\u00e9 mo\u017en\u00e9 pou\u017e\u00edt k v\u00fdrob\u011b fr\u00e9z, kop\u00edrovac\u00edch ty\u010d\u00ed, tv\u00e1\u0159ec\u00edch n\u00e1stroj\u016f bez t\u0159\u00edskov\u00e9ho obr\u00e1b\u011bn\u00ed, rota\u010dn\u00edch razn\u00edk\u016f za studena.<\/p>\n<p>3247 PRIME se m\u016f\u017ee pou\u017e\u00edvat na dal\u0161\u00ed obr\u00e1b\u011bc\u00ed a \u0159ezn\u00e9 n\u00e1stroje, jako jsou vrt\u00e1ky, z\u00e1vitn\u00edky, matrice, v\u0159etena, v\u00fdstru\u017en\u00edky, h\u0159ebeny pro v\u00e1lcov\u00e1n\u00ed z\u00e1vit\u016f, segmenty pro kotou\u010dov\u00e9 pily atd. A tak\u00e9 na v\u00fdstru\u017en\u00edky, st\u0159i\u017en\u00e9 \u010depele nebo v\u00e1lce pro pr\u00e1ci za studena.<\/p>\n<p>3247 PRIME lze d\u00edky vysok\u00e9 tvrdosti za tepla pou\u017e\u00edvat na dutiny a vst\u0159iky plastov\u00fdch forem a v n\u011bkter\u00fdch p\u0159\u00edpadech tak\u00e9 na n\u00e1stroje pro pr\u00e1ci za tepla.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Hlavn\u00ed vlastnosti<\/h3>\n<ul>\n<li>Vynikaj\u00edc\u00ed odolnost proti opot\u0159eben\u00ed<\/li>\n<li>Vysok\u00e1 odolnost proti k\u0159ehnut\u00ed p\u0159i popou\u0161t\u011bn\u00ed<\/li>\n<li>Vysok\u00e1 tvrdost za tepla<\/li>\n<li>Vysok\u00e1 pevnost v tlaku<\/li>\n<li>Vysok\u00e1 prokalitelnost<\/li>\n<\/ul>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Chemick\u00e9 slo\u017een\u00ed <em>(typick\u00e9)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>C<\/th>\n<th>Mn<\/th>\n<th>Si<\/th>\n<th>P<\/th>\n<th>S<\/th>\n<th>Cr<\/th>\n<th>Mo<\/th>\n<th>V<\/th>\n<th>W<\/th>\n<th>Co<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.10<\/td>\n<td>0.20<\/td>\n<td>0.45<\/td>\n<td>\u2264 0.030<\/td>\n<td>\u2264 0.030<\/td>\n<td>3.90<\/td>\n<td>9.40<\/td>\n<td>1.10<\/td>\n<td>1.35<\/td>\n<td>7.95<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h3>Ozna\u010den\u00ed<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>\u010c. materi\u00e1lu<\/th>\n<th>ISO<\/th>\n<th>\u010c\u00edna GB<\/th>\n<th>JIS Japonsko<\/th>\n<th>UK<\/th>\n<th>AISI USA<\/th>\n<th>Rusko Gost<\/th>\n<th>AFNOR<\/th>\n<th>Jin\u00e9 \/ speci\u00e1ln\u00ed<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.3247<\/td>\n<td>HS 2-9-1-8 \/ X110MoCoCrWV 10 8 4 2 1<\/td>\n<td>W2Mo9Cr4VCo8<\/td>\n<td>SKH59<\/td>\n<td>BM42<\/td>\n<td>M42<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Srovn\u00e1n\u00ed jakost\u00ed HSS<\/h3>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<p><img decoding=\"async\" class=\"wp-image-4246\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-srovnavaci-tabulka-hss.png\" alt=\"Srovn\u00e1n\u00ed jakost\u00ed HSS 3343, 3243, 3247 (konven\u010dn\u00ed) a TPM M4, TPM M42, TPM23, TPM30, TPM60 (PM ocel) na desetibodov\u00e9 \u0161k\u00e1le te\u010dkami pro tvrdost za tepla, odolnost proti opot\u0159eben\u00ed, hou\u017eevnatost, obrobitelnost (\u017e\u00edh\u00e1no) a brousitelnost; 3247 m\u00e1 7, 6, 3, 8 a 7 te\u010dek\" width=\"1016\" height=\"378\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-srovnavaci-tabulka-hss.png 1523w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-srovnavaci-tabulka-hss-300x112.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-srovnavaci-tabulka-hss-1024x381.png 1024w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-srovnavaci-tabulka-hss-768x286.png 768w\" sizes=\"auto, (max-width: 1016px) 100vw, 1016px\" \/><\/p>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Struktura<\/h3>\n<p>Struktura materi\u00e1lu 3247 PRIME je jemn\u00e1 a homogenn\u00ed, bez vylou\u010den\u00fdch hrub\u00fdch karbid\u016f nebo jejich shluk\u016f. Rozlo\u017een\u00ed karbid\u016f a mikro\u010distota jsou kontrolov\u00e1ny a jsou ve shod\u011b s normou Stahl-Eisen Werkstoff Blatt 1570 \/ 61.<\/p>\n<p>Velikost austenitick\u00e9ho zrna se stanovuje na povrchu vzorku podle Snyder-Graffovy metody. Minim\u00e1ln\u00ed p\u0159\u00edpustn\u00e9 hodnoty <em>(pr\u016fm\u011br z 10 m\u011b\u0159en\u00ed)<\/em> p\u0159ed popou\u0161t\u011bn\u00edm jsou uvedeny n\u00ed\u017ee.<\/p>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Pr\u016f\u0159ez (mm)<\/th>\n<th>Velikost austenitick\u00e9ho zrna<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>0 &#8211; 25<\/td>\n<td>12<\/td>\n<\/tr>\n<tr>\n<td>25 &#8211; 50<\/td>\n<td>11<\/td>\n<\/tr>\n<tr>\n<td>50 &#8211; 125<\/td>\n<td>10<\/td>\n<\/tr>\n<tr>\n<td>&gt; 125<\/td>\n<td>9<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h3>Tvrdost p\u0159i dod\u00e1n\u00ed<\/h3>\n<p>\u017d\u00edh\u00e1n\u00ed na max. 300 HB.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Fyzik\u00e1ln\u00ed vlastnosti<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Temperature<\/th>\n<th>20\u00b0C<\/th>\n<th>350\u00b0C<\/th>\n<th>700\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Volumic mass kg\/m\u00b3<\/th>\n<td>8120<\/td>\n<td>7930<\/td>\n<td>7725<\/td>\n<\/tr>\n<tr>\n<th>Young Modulus N\/mm\u00b2<\/th>\n<td>220000<\/td>\n<td>200000<\/td>\n<td>178000<\/td>\n<\/tr>\n<tr>\n<th>Thermal conductivity W\/m.K<\/th>\n<td>20<\/td>\n<td>18.7<\/td>\n<td>18.0<\/td>\n<\/tr>\n<tr>\n<th>Coefficient of linear expansion 10<sup>-6<\/sup>\/K<\/th>\n<td>11<\/td>\n<td>12<\/td>\n<td>12.6<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Tepeln\u00e9 zpracov\u00e1n\u00ed<\/h3>\n<h4>M\u011bkk\u00e9 \u017e\u00edh\u00e1n\u00ed<\/h4>\n<p>Teplota: 820 &#8211; 860\u00b0C, doba trv\u00e1n\u00ed 1 h + 1 h pro tlou\u0161\u0165ku 25 mm. pomal\u00e9 chlazen\u00ed v peci <em>(10 a\u017e 20\u00b0C\/h)<\/em>. Atmosf\u00e9ra v peci mus\u00ed b\u00fdt reduk\u010dn\u00ed, aby nedo\u0161lo k oduhli\u010den\u00ed oceli.<\/p>\n<h4>Odstran\u011bn\u00ed pnut\u00ed<\/h4>\n<p>Po opracov\u00e1n\u00ed se doporu\u010duje odstranit pnut\u00ed p\u0159i teplot\u011b 600 &#8211; 650\u00b0C po dobu minim\u00e1ln\u011b 2 hodiny, s n\u00e1sledn\u00fdm pomal\u00fdm ochlazen\u00edm v peci na teplotu 450\u00b0C.<\/p>\n<h4>Austenitizace<\/h4>\n<p>Aby se p\u0159ede\u0161lo riziku poprask\u00e1n\u00ed, doporu\u010duje se p\u0159edeh\u0159\u00edvat ve 3 kroc\u00edch.<\/p>\n<ul>\n<li>1. krok p\u0159edeh\u0159evu: teplota: 500\u00b0C \u010das: 30 s\/mm tlou\u0161\u0165ky<\/li>\n<li>2. krok p\u0159edeh\u0159evu: teplota: 850\u00b0C \u010das: 30 s\/mm tlou\u0161\u0165ky<\/li>\n<li>3. krok p\u0159edeh\u0159evu: teplota: 1050\u00b0C \u010das: 30 s\/mm tlou\u0161\u0165ky<\/li>\n<\/ul>\n<p>Doporu\u010den\u00e1 teplota austenitizace: 1150 &#8211; 1180\u00b0C. Doba v\u00fddr\u017ee nesm\u00ed b\u00fdt p\u0159\u00edli\u0161 dlouh\u00e1, aby se p\u0159ede\u0161lo riziku hrubnut\u00ed zrn a ztr\u00e1t\u011b hou\u017eevnatosti. Jakmile teplota povrchu dos\u00e1hne teploty austenitizace, doporu\u010duje se udr\u017eovat d\u00edl p\u0159i teplot\u011b austenitizace 30 minut na palec tlou\u0161\u0165ky.<\/p>\n<h4>Kalic\u00ed m\u00e9dium<\/h4>\n<p>Olej p\u0159i 80\u00b0C, vakuum <em>(tlak &gt; 6 bar\u016f)<\/em>, soln\u00e1 l\u00e1ze\u0148 500 &#8211; 550\u00b0C.<br \/>\nPro zaji\u0161t\u011bn\u00ed dobr\u00e9 hou\u017eevnatosti je vhodn\u011bj\u0161\u00ed zpracov\u00e1n\u00ed za pou\u017eit\u00ed oleje nebo soln\u00e9 l\u00e1zn\u011b.<br \/>\nPo zakalen\u00ed \u010din\u00ed tvrdost 66 &#8211; 69 HRC.<\/p>\n<h4>Zpracov\u00e1n\u00ed pod bodem mrazu<\/h4>\n<p>U d\u00edl\u016f, kter\u00e9 maj\u00ed m\u00edt vysokou rozm\u011brovou stabilitu a vy\u0161\u0161\u00ed odolnost proti opot\u0159eben\u00ed bez sn\u00ed\u017een\u00ed hou\u017eevnatosti, se doporu\u010duje prov\u00e1d\u011bt zpracov\u00e1n\u00ed pod bodem mrazu p\u0159i teplot\u011b mezi -70\u00b0C a -190\u00b0C po dobu 1 hodiny na 25 mm tlou\u0161\u0165ky d\u00edlu.<\/p>\n<p>Teplotn\u00ed rozsah od -70\u00b0C do -120\u00b0C <em>(tzv. zpracov\u00e1n\u00ed oceli za studena)<\/em> vede k \u00fapln\u00e9 p\u0159em\u011bn\u011b austenitu na martenzit a v d\u016fsledku toho k lep\u0161\u00ed stabilit\u011b ve spojen\u00ed se zv\u00fd\u0161enou tvrdost\u00ed a lep\u0161\u00ed odolnost\u00ed proti opot\u0159eben\u00ed.<\/p>\n<p>Teplotn\u00ed rozsah od -135\u00b0C do -190\u00b0C <em>(tzv. kryogenn\u00ed zpracov\u00e1n\u00ed oceli)<\/em> vede tak\u00e9 k \u00fapln\u00e9 p\u0159em\u011bn\u011b austenitu a d\u00e1le k vylu\u010dov\u00e1n\u00ed ultrajemn\u00fdch karbid\u016f, co\u017e v\u00fdrazn\u011b zvy\u0161uje odolnost proti opot\u0159eben\u00ed beze zm\u011bny hou\u017eevnatosti.<\/p>\n<p>Tato \u00faprava je pro b\u011b\u017en\u00e9 oblasti pou\u017eit\u00ed voliteln\u00e1.<\/p>\n<h4>Popou\u0161t\u011bn\u00ed<\/h4>\n<p>Aby byl obsah zbytkov\u00e9ho austenitu co nejni\u017e\u0161\u00ed a z\u00e1rove\u0148 byla zaji\u0161t\u011bna v\u011bt\u0161\u00ed stabilita n\u00e1stroje, je nezbytn\u00e9 prov\u00e9st dvoj\u00ed <em>(lep\u0161\u00ed je troj\u00ed)<\/em> popou\u0161t\u011bn\u00ed. Po ka\u017ed\u00e9m popou\u0161t\u011bn\u00ed n\u00e1sleduje ochlazen\u00ed pod 100\u00b0C. Doba ka\u017ed\u00e9ho popou\u0161t\u011bn\u00ed mus\u00ed b\u00fdt nejm\u00e9n\u011b 1 h + 1 h na 25 mm tlou\u0161\u0165ky zpracov\u00e1van\u00e9ho d\u00edlu <em>(ekvivalentn\u00ed tepeln\u00e1 tlou\u0161\u0165ka)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<p><img decoding=\"async\" class=\"wp-image-4247\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-popousteci-krivka.png\" alt=\"3247 PRIME popou\u0161t\u011bc\u00ed k\u0159ivka: tvrdost (HRC) v z\u00e1vislosti na teplot\u011b popou\u0161t\u011bn\u00ed (400 a\u017e 650 \u00b0C) pro k\u0159ivky 1160 a 1130 \u00b0C, s maxim\u00e1ln\u00ed tvrdost\u00ed asi 70 HRC kolem 580 \u00b0C\" width=\"520\" height=\"511\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-popousteci-krivka.png 673w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-prime-popousteci-krivka-300x295.png 300w\" sizes=\"auto, (max-width: 520px) 100vw, 520px\" \/><\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Povrchov\u00e1 \u00faprava<\/h3>\n<h4>PVD, CVD<\/h4>\n<p>3247 PRIME se hod\u00ed pro v\u0161echny druhy \u00faprav PVD a CVD, pokud je teplota zpracov\u00e1n\u00ed o 30\u00b0C ni\u017e\u0161\u00ed ne\u017e teplota posledn\u00edho popou\u0161t\u011bn\u00ed.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;60&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h3>Obr\u00e1b\u011bn\u00ed<\/h3>\n<p>N\u00ed\u017ee uveden\u00e9 parametry obr\u00e1b\u011bn\u00ed jsou pouze informativn\u00ed a mus\u00ed b\u00fdt upraveny v z\u00e1vislosti na za\u0159\u00edzen\u00ed a obvykl\u00fdch podm\u00ednk\u00e1ch obr\u00e1b\u011bn\u00ed.<\/p>\n<h4>Brou\u0161en\u00ed v \u017e\u00edhan\u00e9m stavu<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th colspan=\"2\">Karbidov\u00e1 vlo\u017eka<\/th>\n<th>Celistv\u00fd n\u00e1stroj<\/th>\n<\/tr>\n<tr>\n<th><\/th>\n<th>Hrub\u00e9 obr\u00e1b\u011bn\u00ed<\/th>\n<th>\u00bd dokon\u010dovac\u00ed pr\u00e1ce<\/th>\n<th>Dokon\u010dovac\u00ed pr\u00e1ce<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>\u0158ezn\u00e1 rychlost m\/min<\/th>\n<td>50 &#8211; 70<\/td>\n<td>80 &#8211; 105<\/td>\n<td>40 &#8211; 45<\/td>\n<\/tr>\n<tr>\n<th>Posuv mm\/r<\/th>\n<td>0.35<\/td>\n<td>0.15<\/td>\n<td>0.01 &#8211; 0.1<\/td>\n<\/tr>\n<tr>\n<th>Hloubka \u0159ezu mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.01 &#8211; 0.1<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Soustru\u017een\u00ed v \u017e\u00edhan\u00e9m stavu<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th colspan=\"2\">Karbidov\u00e1 vlo\u017eka<\/th>\n<th>N\u00e1stroj z HSS<\/th>\n<\/tr>\n<tr>\n<th><\/th>\n<th>Hrub\u00e9 soustru\u017een\u00ed<\/th>\n<th>Dokon\u010dovac\u00ed pr\u00e1ce<\/th>\n<th>Soustru\u017een\u00ed<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>\u0158ezn\u00e1 rychlost m\/min<\/th>\n<td>90 &#8211; 110<\/td>\n<td>115 &#8211; 130<\/td>\n<td>15<\/td>\n<\/tr>\n<tr>\n<th>Posuv mm\/r<\/th>\n<td>0.35<\/td>\n<td>0.15<\/td>\n<td>0.1 &#8211; 0.2<\/td>\n<\/tr>\n<tr>\n<th>Hloubka \u0159ezu mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.5 &#8211; 2.0<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Vrt\u00e1n\u00ed v \u017e\u00edhan\u00e9m stavu:<br \/>Karbidov\u00fd vrt\u00e1k<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Vlo\u017eka<\/th>\n<th>Slinut\u00fd<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>\u0158ezn\u00e1 rychlost m\/min<\/th>\n<td>120<\/td>\n<td>60<\/td>\n<\/tr>\n<tr>\n<th>Posuv mm\/r<\/th>\n<td>0.10<\/td>\n<td>0.20<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<h4>Spir\u00e1lov\u00fd vrt\u00e1k z HSS<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Pr\u016fm\u011br vrt\u00e1ku mm<\/th>\n<th>\u0158ezn\u00e1 rychlost m\/min<\/th>\n<th>Posuv mm\/r<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>&lt; 5<\/td>\n<td rowspan=\"4\">9<\/td>\n<td>0.10<\/td>\n<\/tr>\n<tr>\n<td>5 &#8211; 10<\/td>\n<td>0.17<\/td>\n<\/tr>\n<tr>\n<td>10 &#8211; 15<\/td>\n<td>0.22<\/td>\n<\/tr>\n<tr>\n<td>15 &#8211; 20<\/td>\n<td>0.30<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Jemn\u00e9 brou\u0161en\u00ed<\/h4>\n<p>Obecn\u00e9 pokyny k pou\u017eit\u00ed brusn\u00fdch kotou\u010d\u016f na 3247 PRIME po tepeln\u00e9m zpracov\u00e1n\u00ed.<\/p>\n<p>Obvykle se pou\u017e\u00edvaj\u00ed sp\u00ed\u0161e m\u011bkk\u00e9 brusn\u00e9 kotou\u010de z vitrifikovan\u00e9ho oxidu hlinit\u00e9ho <em>(t\u0159\u00eddy G pro rovinn\u00e9 brou\u0161en\u00ed a\u017e K pro brou\u0161en\u00ed v\u00e1lcov\u00fdch ploch)<\/em>.<\/p>\n<p>Zvl\u00e1\u0161tn\u00ed pozornost je t\u0159eba v\u011bnovat \u00fa\u010dinn\u00e9mu chlazen\u00ed povrchu b\u011bhem brou\u0161en\u00ed, aby se p\u0159ede\u0161lo degradaci povrchu materi\u00e1lu.<\/p>\n<h4>Elektrojiskrov\u00e9 obr\u00e1b\u011bn\u00ed<\/h4>\n<p>3247 PRIME se hod\u00ed tak\u00e9 k elektrojiskrov\u00e9mu obr\u00e1b\u011bn\u00ed <em>(EDM) (dr\u00e1t nebo elektroda)<\/em>. P\u0159ednostn\u011b se obr\u00e1b\u011bn\u00ed prov\u00e1d\u00ed p\u0159i n\u00edzk\u00e9 proudov\u00e9 hustot\u011b a vysok\u00e9 frekvenci, aby se co mo\u017en\u00e1 nejv\u00edce omezila tlou\u0161\u0165ka b\u00edl\u00e9 vrstvy.<\/p>\n<p>Potom je nutn\u00e9 odstranit pnut\u00ed p\u0159i teplot\u011b 25\u00b0C pod posledn\u00edm popou\u0161t\u011bn\u00edm, aby se sn\u00ed\u017eila \u00farove\u0148 zbytkov\u00fdch nap\u011bt\u00ed <em>(kter\u00e1 by mohla v\u00e9st k riziku vzniku trhlin)<\/em>, a le\u0161t\u011bn\u00ed, aby se zcela odstranila b\u00edl\u00e1 vrstva vznikl\u00e1 b\u011bhem procesu elektrojiskrov\u00e9ho obr\u00e1b\u011bn\u00ed.<\/p>\n<h3>Sva\u0159ov\u00e1n\u00ed<\/h3>\n<p>3247 PRIME nelze sva\u0159ovat.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8220;in_container&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; scene_position=&#8220;center&#8220; bottom_padding=&#8220;120&#8243; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220; column_element_direction_desktop=&#8220;default&#8220; column_element_spacing=&#8220;default&#8220; desktop_text_alignment=&#8220;default&#8220; tablet_text_alignment=&#8220;default&#8220; phone_text_alignment=&#8220;default&#8220; background_color_opacity=&#8220;1&#8243; background_hover_color_opacity=&#8220;1&#8243; column_backdrop_filter=&#8220;none&#8220; column_shadow=&#8220;none&#8220; column_border_radius=&#8220;none&#8220; column_link_target=&#8220;_self&#8220; column_position=&#8220;default&#8220; gradient_direction=&#8220;left_to_right&#8220; overlay_strength=&#8220;0.3&#8243; width=&#8220;1\/1&#8243; tablet_width_inherit=&#8220;default&#8220; animation_type=&#8220;default&#8220; bg_image_animation=&#8220;none&#8220; border_type=&#8220;simple&#8220; column_border_width=&#8220;none&#8220; column_border_style=&#8220;solid&#8220;][vc_column_text css=&#8220;&#8220; text_direction=&#8220;default&#8220;]\n<div style=\"max-width:680px\">\n<p><a href=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/3247-Prime-CS.pdf\" target=\"_blank\" rel=\"noopener\"><strong>St\u00e1hnout produktov\u00fd list 3247 PRIME (PDF)<\/strong><\/a><\/p>\n<p>Dal\u0161\u00ed jakosti: <a href=\"https:\/\/www.tgsteels.com\/cs\/rychlorezne-oceli\/\">Rychlo\u0159ezn\u00e9 oceli<\/a>. Kde koupit: <a href=\"https:\/\/www.tgsteels.com\/cs\/servisni-centra\/\">Servisn\u00ed centra<\/a>.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row]\n","protected":false},"excerpt":{"rendered":"<p>[vc_row type=&#8220;full_width_background&#8220; full_screen_row_position=&#8220;middle&#8220; column_margin=&#8220;default&#8220; column_direction=&#8220;default&#8220; column_direction_tablet=&#8220;default&#8220; column_direction_phone=&#8220;default&#8220; video_bg=&#8220;use_video&#8220; video_mp4=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.mp4&#8243; video_webm=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.webm&#8220; video_ogv=&#8220;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero.ogv&#8220; background_video_loading=&#8220;default&#8220; scene_position=&#8220;center&#8220; text_color=&#8220;dark&#8220; text_align=&#8220;left&#8220; row_border_radius=&#8220;none&#8220; row_border_radius_applies=&#8220;bg&#8220; overflow=&#8220;visible&#8220; overlay_strength=&#8220;0.3&#8243; gradient_direction=&#8220;left_to_right&#8220; shape_divider_position=&#8220;bottom&#8220; bg_image_animation=&#8220;none&#8220; parallax_bg=&#8220;true&#8220; parallax_bg_speed=&#8220;fast&#8220; gradient_type=&#8220;default&#8220; shape_type=&#8220;&#8220;][vc_column column_padding=&#8220;no-extra-padding&#8220; column_padding_tablet=&#8220;inherit&#8220; column_padding_phone=&#8220;inherit&#8220; column_padding_position=&#8220;all&#8220;&#8230;<\/p>\n","protected":false},"author":6,"featured_media":0,"parent":2703,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"inline_featured_image":false,"footnotes":""},"class_list":["post-4294","page","type-page","status-publish"],"_links":{"self":[{"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/pages\/4294","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/comments?post=4294"}],"version-history":[{"count":1,"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/pages\/4294\/revisions"}],"predecessor-version":[{"id":4373,"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/pages\/4294\/revisions\/4373"}],"up":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/pages\/2703"}],"wp:attachment":[{"href":"https:\/\/www.tgsteels.com\/cs\/wp-json\/wp\/v2\/media?parent=4294"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}