Very high toughness cold work tool steel with simple heat treatment
2842 PRIME;
- is a medium-alloyed, oil-hardenable, cold-worked steel with low deformability and 2% manganese.
- has good wear resistance associated with good toughness.
- has good dimensional stability during heat treatment.
Applications
2842 PRIME can be used for blanking and forming dies, back plates, punches and pins for forming steel parts up to 6 mm thick.
2842 PRIME can also be used for industrial knives for the wood, paper and metal industry.
2842 PRIME can be used for cold cutting shear blades for shear steel plates up to 6 mm thick.
2842 PRIME can be used for the manufacture of cutting and punching tools up to 6mm thick. It can also be used for the manufacture of taps, slides, gauges, guide columns, as well as for highly abrasive plastic mold cavities and gates.
Main properties
- Good toughness and good wear resistance
- High resistance to cracking
- Very good machinability
- Simple heat treatment with high dimensional stability
- Suitable for surface treatments
Chemical composition (typical)
| C | Mn | Si | P | S | Cr | Mo | V |
|---|---|---|---|---|---|---|---|
| 0.90 | 2.00 | 0.25 | ≤ 0.030 | ≤ 0.005 | 0.35 | – | 0.15 |
Designation
| Werkstoff Nr | ISO | China GB | JIS Japan | UK | AISI USA | Russia Gost | AFNOR | Other / Special |
|---|---|---|---|---|---|---|---|---|
| 1.2842 | 90MnCrV8 | 9Mn2V | – | – | O2 | – | – | – |
Structure
The structure of the 2842 PRIME is fine and homogeneous without precipitation or alignments of carbides.
Hardness at the time of delivery
Annealed for 230 HB max.
Physical properties
| Temperature | 20°C | 300°C | 600°C |
|---|---|---|---|
| Volumic mass kg/m³ | 7700 | 7680 | – |
| Young Modulus N/mm² | 210000 | 187000 | – |
| Thermal conductivity W/m.K | 33 | 32 | 31 |
| Coefficient of linear expansion 10-6/K | 12 | 13.9 | 15 |
Heat treatment
Soft annealing
Temperature: 690 – 720°C, duration 1h + 1h for 25mm thickness. slow cooling in the furnace (10 to 20°C/h). The atmosphere in the furnace must be reducing to avoid decarburization of the steel.
Stress relieving
After machining, it is recommended to perform stress relieving at 600 – 650°C (always at temperature never exceeding 50°C below the tempering temperature) for a minimum of 2 hours, followed by slow cooling in the furnace to 450°C.
Austenitization
In order to avoid any risk of cracking it is recommended to preheat in 1 step.
- 1st preheating step: temperature: 550°C time: 30 s/mm of thickness
Recommended austenitizing temperature: 800 – 820°C. The holding time should not be too long to avoid a risk of grain coarsening and a loss of toughness. It is recommended to keep the part at the austenitizing temperature 30 minutes per inch of thickness as soon as the temperature of the surface reach the austenitization temperature.
Quenching medium
Oil at 80°C, vacuum (pressure > 6 bars), salt bath 500 – 550°C.
To ensure good toughness, treatment with oil or salt bath is preferable.
After quenching the hardness is 60 – 63 HRC
Sub zero treatment
For parts that need to have high dimensional stability and to increase wear resistance without reducing toughness, it is recommended to perform a subzero treatment at a temperature between -70°C and -120°C for 1 hour for 25 mm of thickness of the part.
The temperature range from -70°C up to -120°C (named cold treatment of steel) leads to the complete transformation of austenite into martensite and as a consequence to a better stability associated with an improved hardness and a better wear resistance.This treatment is optional for common applications.
Tempering
To ensure a minimum residual austenite rate as well as greater tool stability, it is essential to perform a double (triple is better) tempering. Each tempering is followed by a cooling under 100°C. Each tempering time must be at least equal to 1h + 1h for 25 mm of thickness of the treated part (equivalent thermal thickness).

Surface treatment
PVD, CVD
2842 PRIME is suitable for all kinds of PVD and CVD treatment as soon as the treatment temperature is 30°C lower than the last tempering temperature.
Polishing
2842 PRIME is perfectly suitable for polishing in the treated state and can be used for applications requiring a sufficiently high polish level for translucent – transparent parts (Rt ≤ 20 µm, CNOMO level 2, Rugotest N7).
Optimal polishing is achieved by performing consecutive steps of fairly close roughness and stopping each step as soon as the last scratch of the previous step disappears
Machining
The machining parameters below are given for information only and must be adapted according to the equipment and usual machining conditions.
Note: the cutting parameters are similar to those of the 2510 PRIME but since there is no tungsten in the composition of the 2842 PRIME the wear of the tools used for machining 2842 PRIME is less important than for machining 2510 PRIME.
Turning
| Carbide tool Rough machining |
Carbide tool Finishing |
HSS tool Finishing |
|
|---|---|---|---|
| Cutting speed m/min | 150 – 200 | 200 – 250 | 20 – 25 |
| Feed mm/r | 0.2 – 0.4 | 0.1 – 0.2 | 0.1 – 0.2 |
| Depth of cut mm | 2 – 4 | 0.5 – 2 | 0.5 – 2 |
Grinding in annealed conditions
| Milling with carbide tools Rough machining |
Milling with carbide tools ½ Finishing |
Solid tool Finishing |
|
|---|---|---|---|
| Cutting speed m/min | 160 – 230 | 260 – 280 | 160 – 180 |
| Feed mm/r | 0.2 – 0.4 | 0.1 – 0.2 | 0.02 – 0.2 |
| Depth of cut mm | 2 – 4 | 1 – 2 |
Drilling: carbide drill
| Carbide type | Indexable insert | Solid carbide | Carbide tip |
|---|---|---|---|
| Cutting speed m/min | 200 – 230 | 105 – 135 | 65 – 85 |
| Feed mm/t | 0.05 – 0.15 | 0.10 – 0.25 | 0.15 – 0.25 |
Drilling: HSS twist drill
| Drill diameter mm | Cutting speed m/min | Feed mm/t |
|---|---|---|
| < 5 | 14 – 16 | 0.10 – 0.20 |
| 5 – 10 | 14 – 16 | 0.20 – 0.30 |
| 10 – 15 | 14 – 16 | 0.30 – 0.35 |
| 15 – 20 | 14 – 16 | 0.35 – 0.40 |
Fine grinding
General indications for grinding wheels to be used on 2842 PRIME in the heat treated condition
Usually, rather soft vitrified aluminum oxide grinding wheels (grades G for plane grinding to K for cylindrical grinding) are used.
Particular attention will be paid to effective cooling of the surface during grinding to prevent degradation of the material surface.
Electro-discharge machining
2842 PRIME is also suitable for EDM machining (wire or electrode). Preferably, the machining will be carried out with a low current density and a high frequency in order to limit the thickness of the white layer as much as possible.
Then it is necessary to carry out a stress relieving at 25°C below the last tempering in order to reduce the level of residual stresses (which could lead to a risk of cracking) and to carry out a polishing to completely remove the white layer formed during the discharge machining process.
Welding
2842 PRIME could be welded either in the annealed condition (better) or in the heat treated condition.
- Method: TIG
- Feeder wire: AISI O2 or AWS312
- Preheating: 250°C. Hold at 200°C during the welding operation
- Post treatment:
- In the treated state: tempering for a minimum of 2 hours at 20°C below the initial tempering temperature
- In the annealed state: carry out a soft annealing under the usual conditions: temperature: 740 – 770°C, duration 1h + 1h for 25 mm of thickness. Slow cooling in the oven (10 to 20°C/h).
Download the 2842 PRIME datasheet (PDF)
More grades: Cold Work Tool Steels. Where to buy: Service Network.