{"id":4075,"date":"2026-10-08T14:31:10","date_gmt":"2026-10-08T14:31:10","guid":{"rendered":"https:\/\/www.tgsteels.com\/cold-work-tool-steels\/2360-prime\/"},"modified":"2026-10-08T15:38:33","modified_gmt":"2026-10-08T15:38:33","slug":"2360-prime","status":"publish","type":"page","link":"https:\/\/www.tgsteels.com\/en\/cold-work-tool-steels\/2360-prime\/","title":{"rendered":"2360 PRIME"},"content":{"rendered":"[vc_row type=&#8221;full_width_background&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; video_bg=&#8221;use_video&#8221; video_mp4=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&#8243; video_webm=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm&#8221; video_ogv=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv&#8221; background_video_loading=&#8221;default&#8221; scene_position=&#8221;center&#8221; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; parallax_bg=&#8221;true&#8221; parallax_bg_speed=&#8221;fast&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/2&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221; column_padding_type=&#8221;default&#8221; gradient_type=&#8221;default&#8221;][divider line_type=&#8221;No Line&#8221; custom_height=&#8221;450&#8243;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<h1>2360 PRIME <span style=\"display:block;font-size:.5em;line-height:1.35;margin-top:.4em\">(1.2360, X48CrMoV8-1-1)<\/span><\/h1>\n[\/vc_column_text][divider line_type=&#8221;No Line&#8221; custom_height=&#8221;50&#8243;][\/vc_column][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/2&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h4>Tool steel for cold and hot work applications where high strength and hardness are combined with high toughness<\/h4>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p>2360 PRIME is a special alloyed Cr-Mo-V steel, secondarily hardenable, with very high toughness, good compressive strength, high wear resistance also at high temperatures.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Applications<\/h3>\n<p>2360 PRIME can be used for hot working: applications as hot stamping dies, press hardening dies for direct and indirect methods.<\/p>\n<p>2360 PRIME can be used for all cold working applications requiring a combination of high hardness and toughness as in in automotive and white goods industries.<\/p>\n<p>2360 PRIME can be used for industrial Knives and it is especially suitable for a use as chipping knives and all industrial knives such as those in the paper and wood industry and also for knives for cutting metals thicker than 5 mm.<\/p>\n<p>If higher polish ability is required <em>(e.g. for mirror polish or higher toughness)<\/em> we recommend to use the <a href=\"https:\/\/www.tgsteels.com\/en\/cold-work-tool-steels\/tgx-snapper-esr\/\">SNAPPER ESR<\/a> <em>(remelted steel with the highest cleanliness)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Main properties<\/h3>\n<ul>\n<li>Excellent wear resistance even at high temperatures<\/li>\n<li>Very good toughness<\/li>\n<li>Good compressive strength<\/li>\n<li>High hardenability<\/li>\n<\/ul>\n<h3>Chemical composition <em>(typical)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>C<\/th>\n<th>Mn<\/th>\n<th>Si<\/th>\n<th>P<\/th>\n<th>S<\/th>\n<th>Cr<\/th>\n<th>Mo<\/th>\n<th>V<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>0.47<\/td>\n<td>0.50<\/td>\n<td>0.80<\/td>\n<td>\u2264 0.02<\/td>\n<td>\u2264 0.003<\/td>\n<td>7.55<\/td>\n<td>1.50<\/td>\n<td>1.40<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Designation<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Werkstoff Nr<\/th>\n<th>ISO<\/th>\n<th>China GB<\/th>\n<th>JIS Japan<\/th>\n<th>UK<\/th>\n<th>AISI USA<\/th>\n<th>Russia Gost<\/th>\n<th>AFNOR<\/th>\n<th>Other \/ Special<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.2360<\/td>\n<td>X48CrMoV8-1-1<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<p><img decoding=\"async\" class=\"wp-image-4037\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram.png\" alt=\"Positioning diagram of toughness (vertical axis) versus wear resistance (horizontal axis) comparing 2360 PRIME with 1.2550, 1.2363, 1.3343, 1.2379 and the TGX, TPM and TG Wear grades\" width=\"1016\" height=\"455\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram.png 1639w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram-300x134.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram-1024x459.png 1024w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram-768x344.png 768w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-wear-toughness-diagram-1536x688.png 1536w\" sizes=\"auto, (max-width: 1016px) 100vw, 1016px\" \/><\/p>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Structure<\/h3>\n<p>Because of the moderate carbon content and the medium chromium content the structure of the 2360 PRIME is fine and homogeneous without precipitation or alignments of carbides.<\/p>\n<h3>Hardness at the time of delivery<\/h3>\n<p>Annealed for 250 HB max.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Physical properties<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Temperature<\/th>\n<th>20\u00b0C<\/th>\n<th>200\u00b0C<\/th>\n<th>400\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Volumic mass kg\/m<sup>3<\/sup><\/th>\n<td>7800<\/td>\n<td>7750<\/td>\n<td>7700<\/td>\n<\/tr>\n<tr>\n<th>Young Modulus N\/mm\u00b2<\/th>\n<td>210000<\/td>\n<td>200 000<\/td>\n<td>188000<\/td>\n<\/tr>\n<tr>\n<th>Thermal conductivity W\/m.K<\/th>\n<td>26<\/td>\n<td>24<\/td>\n<td>27<\/td>\n<\/tr>\n<tr>\n<th>Coefficient of linear expansion 10<sup>-6<\/sup>\/K<\/th>\n<td>11.5<\/td>\n<td>11.9<\/td>\n<td>12.5<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Heat treatment<\/h3>\n<h4>Soft annealing<\/h4>\n<p>Temperature: 820 &#8211; 850\u00b0C, duration 1h + 1h for 25 mm thickness. Slow cooling in the furnace <em>(10 to 20\u00b0C\/h)<\/em>. The atmosphere in the furnace must be reducing to avoid decarburization of the steel.<\/p>\n<h4>Stress relieving<\/h4>\n<p>After machining, it is recommended to perform stress relieving at 650\u00b0C for a minimum of 2 hours, followed by slow cooling in the furnace to 450\u00b0C.<\/p>\n<h4>Austenitization<\/h4>\n<p>In order to avoid any risk of cracking it is recommended to preheat in 2 steps.<\/p>\n<ul>\n<li>1st preheating step: temperature: 600\u00b0C time: 30 s\/mm of thickness<\/li>\n<li>2nd preheating step: temperature: 850\u00b0C time: 30 s\/mm of thickness<\/li>\n<\/ul>\n<p>Recommended austenitizing temperature: 1030 &#8211; 1090\u00b0C. The holding time should not be too long to avoid a risk of grain coarsening and a loss of toughness. It is recommended to keep the part at the austenitizing temperature 30 minutes per inch of thickness as soon as the temperature of the surface reach the austenitization temperature.<\/p>\n<h4>Sub zero treatment<\/h4>\n<p>For parts that need to have high dimensional stability and to increase wear resistance without reducing toughness, it is recommended to perform a subzero treatment at a temperature between -70\u00b0C and -190\u00b0C for 1 hour for 25 mm of thickness of the part. The temperature range from -70\u00b0C up to -120\u00b0C <em>(named cold treatment of steel)<\/em> leads to the complete transformation of austenite into martensite and as a consequence to better stability associated with improved hardness and better wear resistance and the temperature range from -135\u00b0C down to -190\u00b0C <em>(named cryotreatment of steel)<\/em> leads also to the complete transformation of austenite and also the precipitation of ultrafine carbides improving a lot the wear resistance without modification of the toughness.<\/p>\n<p>This treatment is optional for common applications.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h4>Quenching medium<\/h4>\n<p>Oil at 80\u00b0C, vacuum <em>(pressure &gt; 6 bars)<\/em>, salt bath 500 &#8211; 550\u00b0C.<br \/>\nTo ensure good toughness, treatment with oil or salt bath is preferable.<br \/>\nThe hardness after quenching is 54 to 56 HRC.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p><img decoding=\"async\" class=\"wp-image-4038\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-tempering-curve.png\" alt=\"2360 PRIME tempering curve: hardness (HRC) versus tempering temperature (\u00b0C), about 60 HRC at low tempering temperatures, a secondary hardness peak near 500 \u00b0C and a fall to about 30 HRC at 700 \u00b0C\" width=\"520\" height=\"502\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-tempering-curve.png 710w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/2360-prime-tempering-curve-300x289.png 300w\" sizes=\"auto, (max-width: 520px) 100vw, 520px\" \/><\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h4>Tempering<\/h4>\n<p>To ensure a minimum residual austenite rate as well as greater tool stability, it is essential to perform a double tempering. Each tempering is followed by a cooling under 100\u00b0C.<\/p>\n<p>Each tempering time must be at least equal to 1h + 1h for 25 mm of thickness of the treated part <em>(equivalent thermal thickness)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Surface treatment<\/h3>\n<h4>Nitriding<\/h4>\n<p>2360 PRIME is not recommended to be nitrided since the nitriding temperature of the 2360 PRIME is quite low.<\/p>\n<h4>PVD, CVD<\/h4>\n<p>2360 PRIME is suitable for all kind of PVD and CVD treatment as soon as the treatment temperature is 30\u00b0C lower than the last tempering temperature.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Machining<\/h3>\n<p>The machining parameters below are given for information only and must be adapted according to the equipment and usual machining conditions.<\/p>\n<h4>Turning<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Carbide tool<br \/>Rough machining<\/th>\n<th>Carbide tool<br \/>Finishing<\/th>\n<th>HSS tool<br \/>Finishing<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>130 &#8211; 170<\/td>\n<td>170 &#8211; 220<\/td>\n<td>17 &#8211; 22<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/r<\/th>\n<td>0.15 &#8211; 0.3<\/td>\n<td>0.1 &#8211; 0.15<\/td>\n<td>0.1 &#8211; 0.3<\/td>\n<\/tr>\n<tr>\n<th>Depth of cut mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>0.5 &#8211; 1.5<\/td>\n<td>0.5 &#8211; 2<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Milling: surfacing<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Milling with carbide tools<br \/>Rough machining<\/th>\n<th>Milling with carbide tools<br \/>\u00bd Finishing<\/th>\n<th>Solid tool<br \/>Finishing<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>160 &#8211; 180<\/td>\n<td>180 &#8211; 200<\/td>\n<td>210 &#8211; 280<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/r<\/th>\n<td>0.40<\/td>\n<td>0.4 &#8211; 0.35<\/td>\n<td>0.10 &#8211; 0.05<\/td>\n<\/tr>\n<tr>\n<th>Depth of cut mm<\/th>\n<td>1 &#8211; 2.5<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>1 &#8211; 0.5<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Drilling: HSS twist drill<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Drill diameter mm<\/th>\n<th>Cutting speed m\/min<\/th>\n<th>Feed mm\/t<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>&lt; 5<\/td>\n<td>13 &#8211; 15<\/td>\n<td>0.05 &#8211; 0.15<\/td>\n<\/tr>\n<tr>\n<td>5 &#8211; 10<\/td>\n<td>13 &#8211; 15<\/td>\n<td>0.15 &#8211; 0.20<\/td>\n<\/tr>\n<tr>\n<td>10 &#8211; 15<\/td>\n<td>13 &#8211; 15<\/td>\n<td>0.20 &#8211; 0.25<\/td>\n<\/tr>\n<tr>\n<td>15 &#8211; 20<\/td>\n<td>13 &#8211; 15<\/td>\n<td>0.25 &#8211; 0.30<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Drilling: carbide drill<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Carbide type<\/th>\n<th>Indexable insert<\/th>\n<th>Solid carbide<\/th>\n<th>Carbide tip<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>160 &#8211; 180<\/td>\n<td>100 &#8211; 130<\/td>\n<td>55 &#8211; 80<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/t<\/th>\n<td>0.05 &#8211; 0.10<\/td>\n<td>0.10 &#8211; 0.25<\/td>\n<td>0.15 &#8211; 0.25<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h4>Fine grinding<\/h4>\n<p>General indications for grinding wheels to be used on 2360 PRIME in the heat treated condition<\/p>\n<p>Usually, rather soft vitrified aluminum oxide grinding wheels <em>(grades G for plane grinding to K for cylindrical grinding)<\/em> are used.<\/p>\n<p>Particular attention will be paid to effective cooling of the surface during grinding to prevent degradation of the material surface.<\/p>\n<h4>Electro-discharge machining<\/h4>\n<p>2360 PRIME is also suitable for EDM machining <em>(wire or electrode)<\/em>. Preferably, the machining will be carried out with a low current density and a high frequency in order to limit the thickness of the white layer as much as possible.<\/p>\n<p>Then it is necessary to carry out a stress relieving at 25\u00b0C below the last tempering in order to reduce the level of residual stresses <em>(which could lead to a risk of cracking)<\/em> and to carry out a polishing to completely remove the white layer formed during the discharge machining process.<\/p>\n<h3>Welding<\/h3>\n<p>It is not recommended to weld 2360 PRIME but if this is mandatory it could be welded in the heat treated condition.<\/p>\n<ul>\n<li>Method: TIG<\/li>\n<li>Feeder wire: UTP 67 <em>(56HRC)<\/em> or UTP69 <em>(62 HRC)<\/em><\/li>\n<li>Preheating: 250\u00b0C.<br \/>\nHold at 200\u00b0C during the welding operation with a maximum interpass temperature at 350\u00b0C. Slow cooling <em>(max 20\u00b0C\/h)<\/em> after welding.<\/li>\n<li>Post treatment: tempering at 20\u00b0C below the last tempering temperature with a tempering time at least equal to 1h + 1h for 25 mm of thickness of the treated part <em>(equivalent thermal thickness)<\/em>.<\/li>\n<\/ul>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;120&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p><a href=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/02\/2360-PRIME.pdf\" target=\"_blank\" rel=\"noopener\"><strong>Download the 2360 PRIME datasheet (PDF)<\/strong><\/a><\/p>\n<p>More grades: <a href=\"https:\/\/www.tgsteels.com\/en\/cold-work-tool-steels\/\">Cold Work Tool Steels<\/a>. Where to buy: <a href=\"https:\/\/www.tgsteels.com\/en\/service-network\/\">Service Network<\/a>.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row]\n","protected":false},"excerpt":{"rendered":"<p>[vc_row type=&#8221;full_width_background&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; video_bg=&#8221;use_video&#8221; video_mp4=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&#8243; video_webm=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm&#8221; video_ogv=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv&#8221; background_video_loading=&#8221;default&#8221; scene_position=&#8221;center&#8221; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; parallax_bg=&#8221;true&#8221; parallax_bg_speed=&#8221;fast&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221;&#8230;<\/p>\n","protected":false},"author":6,"featured_media":0,"parent":546,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"inline_featured_image":false,"footnotes":""},"class_list":["post-4075","page","type-page","status-publish"],"_links":{"self":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4075","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/comments?post=4075"}],"version-history":[{"count":1,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4075\/revisions"}],"predecessor-version":[{"id":4151,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4075\/revisions\/4151"}],"up":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/546"}],"wp:attachment":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/media?parent=4075"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}