{"id":4080,"date":"2026-10-08T14:31:40","date_gmt":"2026-10-08T14:31:40","guid":{"rendered":"https:\/\/www.tgsteels.com\/cold-work-tool-steels\/tpm-23-ultraclean\/"},"modified":"2026-10-29T09:57:17","modified_gmt":"2026-10-29T09:57:17","slug":"tpm-23-ultraclean","status":"publish","type":"page","link":"https:\/\/www.tgsteels.com\/en\/cold-work-tool-steels\/tpm-23-ultraclean\/","title":{"rendered":"TPM 23 Ultraclean"},"content":{"rendered":"[vc_row type=&#8221;full_width_background&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; video_bg=&#8221;use_video&#8221; video_mp4=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&#8243; video_webm=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm&#8221; video_ogv=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv&#8221; background_video_loading=&#8221;default&#8221; scene_position=&#8221;center&#8221; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; parallax_bg=&#8221;true&#8221; parallax_bg_speed=&#8221;fast&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/2&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221; column_padding_type=&#8221;default&#8221; gradient_type=&#8221;default&#8221;][divider line_type=&#8221;No Line&#8221; custom_height=&#8221;450&#8243;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<h1>TPM 23 Ultraclean<\/h1>\n[\/vc_column_text][divider line_type=&#8221;No Line&#8221; custom_height=&#8221;50&#8243;][\/vc_column][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/2&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h4>PM HSS for cutting tools and dies<\/h4>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p>TPM23 UltraClean is a high-speed tool steel obtained by powder metallurgy. It is characterized by very good toughness and good wear resistance.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Applications<\/h3>\n<p>TPM23 UltraClean also finds numerous applications in the field of cold work tools for cutting, stamping, spinning as well as for punches or dies.<\/p>\n<p>TPM23 UltraClean can also be used for cold working rollers and also for electrodes in ultrasonic welding machines.<\/p>\n<p>TPM23 UltraClean is used for cutting tools <em>(milling cutters, spindles, knives, etc.)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Main properties<\/h3>\n<ul>\n<li>Very good toughness<\/li>\n<li>Good compressive strength<\/li>\n<li>Good wear resistance<\/li>\n<\/ul>\n<p>Comparison with the other PM tool steels available at TG Steels, the position on the toughness vs wear resistance diagram is shown here under.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Chemical composition <em>(typical)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>C<\/th>\n<th>W<\/th>\n<th>Mo<\/th>\n<th>Cr<\/th>\n<th>V<\/th>\n<th>Co<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.30<\/td>\n<td>6.40<\/td>\n<td>5.00<\/td>\n<td>4.10<\/td>\n<td>3.00<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h3>Designation<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Werkstoff Nr<\/th>\n<th>ISO<\/th>\n<th>China GB<\/th>\n<th>JIS Japan<\/th>\n<th>UK<\/th>\n<th>AISI USA<\/th>\n<th>Russia Gost<\/th>\n<th>AFNOR<\/th>\n<th>Other \/ Special<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.3344 \/ 1.3395<\/td>\n<td>PM HS 6-5-3 \/ X130WMoCrV6-5-4-3<\/td>\n<td>CW6Mo5Cr4V3<\/td>\n<td>PM SKH53<\/td>\n<td>BM3 class 2<\/td>\n<td>PM M 3-2<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><img decoding=\"async\" class=\"wp-image-4048\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram.png\" alt=\"Positioning diagram of the PM tool steels available at TG Steels, toughness (vertical axis) versus wear resistance (horizontal axis); TPM 23 is plotted at medium wear resistance and medium toughness, next to TPM M4\" width=\"1016\" height=\"411\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram.png 1538w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram-300x121.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram-1024x414.png 1024w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram-768x311.png 768w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-wear-toughness-diagram-1536x621.png 1536w\" sizes=\"auto, (max-width: 1016px) 100vw, 1016px\" \/><\/p>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Comparison HSS grades<\/h3>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<p><img decoding=\"async\" class=\"wp-image-4049\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-hss-comparison-table.png\" alt=\"Comparison of HSS grades 3343, 3243, 3247 (conventional) and TPM M4, TPM M42, TPM23, TPM30, TPM60 (PM steel) on a 10-dot scale for hot hardness, wear resistance, toughness, machinability (annealed) and grindability; TPM23 scores 6, 6, 10, 9 and 8 dots\" width=\"1016\" height=\"374\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-hss-comparison-table.png 1514w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-hss-comparison-table-300x110.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-hss-comparison-table-1024x377.png 1024w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-hss-comparison-table-768x283.png 768w\" sizes=\"auto, (max-width: 1016px) 100vw, 1016px\" \/><\/p>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Structure<\/h3>\n<p>The structure of the TPM23 UltraClean is fine and homogeneous without precipitation or alignments of carbides.<\/p>\n<p>Due to its elaboration by powder metallurgy with Hot Isostatic Compression the typical size of the carbides is about 2 \u00b5m and the level of cleanliness is far better than conventional cold work tool steels.<\/p>\n<h3>Hardness at the time of delivery<\/h3>\n<p>Annealed for 270 HB max.<\/p>\n<h3>Typical mechanical properties in hardened conditions <em>(results from internal tests not indicated on the certificates)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Hardness<\/th>\n<th>Compressive yield strength MPa<\/th>\n<th>Impact test unnotched probe J at 23\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>60<\/td>\n<td>2400<\/td>\n<td>60<\/td>\n<\/tr>\n<tr>\n<td>62<\/td>\n<td>2700<\/td>\n<td>50<\/td>\n<\/tr>\n<tr>\n<td>64<\/td>\n<td>3000<\/td>\n<td>40<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Physical properties<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Temperature<\/th>\n<th>20\u00b0C<\/th>\n<th>400\u00b0C<\/th>\n<th>600\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Volumic mass kg\/m\u00b3<\/th>\n<td>8<\/td>\n<td>7770<\/td>\n<td>7700<\/td>\n<\/tr>\n<tr>\n<th>Young Modulus N\/mm\u00b2<\/th>\n<td>225000<\/td>\n<td>207000<\/td>\n<td>183000<\/td>\n<\/tr>\n<tr>\n<th>Thermal conductivity W\/m.K<\/th>\n<td>25<\/td>\n<td>29<\/td>\n<td>27<\/td>\n<\/tr>\n<tr>\n<th>Coefficient of linear expansion 10<sup>-6<\/sup>\/K<\/th>\n<td>12<\/td>\n<td>12.2<\/td>\n<td>12.6<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Heat treatment<\/h3>\n<h4>Soft annealing<\/h4>\n<p>Temperature: 850 &#8211; 900\u00b0C, duration 1h + 1h for 25 mm thickness. Slow cooling in the furnace <em>(10 to 20\u00b0C\/h)<\/em>. The atmosphere in the furnace must be reducing to avoid decarburization of the steel.<\/p>\n<h4>Stress relieving<\/h4>\n<p>After machining, it is recommended to perform stress relieving at 650\u00b0C for a minimum of 2 hours, followed by slow cooling in the furnace to 450\u00b0C.<\/p>\n<h4>Austenitization<\/h4>\n<p>In order to avoid any risk of cracking it is recommended to preheat in 3 steps.<\/p>\n<ul>\n<li>1st preheating step: temperature: 400\u00b0C time: 30 s\/mm of thickness<\/li>\n<li>2nd preheating step: temperature: 850\u00b0C time: 30 s\/mm of thickness<\/li>\n<li>3rd preheating step: temperature: 1050\u00b0C time: 30 s\/mm of thickness<\/li>\n<\/ul>\n<p>Recommended austenitizing temperature: 1140 &#8211; 1150\u00b0C. The holding time should not be too long to avoid a risk of grain coarsening and a loss of toughness. It is recommended to keep the part at the austenitizing temperature 30 minutes per inch of thickness as soon as the temperature of the surface reach the austenitization temperature.<\/p>\n<h4>Quenching medium<\/h4>\n<p>Oil at 80\u00b0C, vacuum <em>(pressure &gt; 6 bars)<\/em>, salt bath 500 &#8211; 550\u00b0C.<br \/>\nTo ensure good toughness, treatment with oil or salt bath is preferable.<\/p>\n<h4>Sub zero treatment<\/h4>\n<p>For parts that need to have high dimensional stability and to increase wear resistance without reducing toughness, it is recommended to perform a subzero treatment at a temperature between -70\u00b0C and -190\u00b0C for 1 hour for 25 mm of thickness of the part.<\/p>\n<p>The temperature range from -70\u00b0C up to -120\u00b0C <em>(named cold treatment of steel)<\/em> leads to the complete transformation of austenite into martensite and as a consequence to better stability associated with improved hardness and better wear resistance and the temperature range from -135\u00b0C down to -190\u00b0C <em>(named cryotreatment of steel)<\/em> leads also to the complete transformation of austenite and also the the precipitation of ultrafine carbides improving a lot the wear resistance without modification of the toughness. This treatment is optional for common applications.<\/p>\n<h4>Tempering<\/h4>\n<p>To ensure a minimum residual austenite rate as well as greater tool stability, it is essential to perform double <em>(better triple)<\/em> tempering. Each tempering is followed by a cooling under 100\u00b0C. Depending on the use of the final part the following tempering temperatures are recommended:<\/p>\n<\/div>\n[\/vc_column_text]\n<table>\n<thead>\n<tr>\n<th>Austenitizing temperature<\/th>\n<th>Tempering temperature<\/th>\n<th>Hardness<\/th>\n<th>Properties<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td rowspan=\"3\">1140 \/ 1150\u00b0C<\/td>\n<td>520\u00b0C<\/td>\n<td>63 \/ 68 HRC<\/td>\n<td>Better wear resistance<\/td>\n<\/tr>\n<tr>\n<td>550\u00b0C<\/td>\n<td>63 \/ 65 HRC<\/td>\n<td>Wear and toughness<\/td>\n<\/tr>\n<tr>\n<td>560\u00b0C<\/td>\n<td>62 \/ 64 HRC<\/td>\n<td>Better toughness<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p>Each tempering time must be at least equal to 1h + 1h for 25 mm of thickness of the treated part <em>(equivalent thermal thickness)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p><img decoding=\"async\" class=\"wp-image-4050\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-tempering-curve.png\" alt=\"TPM 23 Ultraclean tempering curve: hardness (HRC) versus tempering temperature (500 to 600 \u00b0C) after austenitizing in vacuum at 1050, 1100, 1150 and 1180 \u00b0C (3 \u00b0C\/s)\" width=\"520\" height=\"509\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-tempering-curve.png 688w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-23-ultraclean-tempering-curve-300x293.png 300w\" sizes=\"auto, (max-width: 520px) 100vw, 520px\" \/><\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Surface treatment<\/h3>\n<h4>Nitriding<\/h4>\n<p>TPM23 UltraClean can be nitrided at temperatures less than or equal to 20\u00b0C below tempering temperatures without risk of deterioration of the mechanical characteristics.<\/p>\n<h4>PVD, CVD<\/h4>\n<p>3343 PRIME is suitable for all kinds of PVD and CVD treatment as soon as the treatment temperature is 30\u00b0C lower than the last tempering temperature.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;60&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<h3>Machining<\/h3>\n<p>The machining parameters below are given for information only and must be adapted according to the equipment and usual machining conditions<\/p>\n<h4>Grinding in annealed conditions<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Carbide insert<br \/>Rough machining<\/th>\n<th>Carbide insert<br \/>\u00bd Finishing<\/th>\n<th>Solid tool<br \/>Finishing<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>110 &#8211; 130<\/td>\n<td>125 &#8211; 160<\/td>\n<td>40 &#8211; 50<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/r<\/th>\n<td>0.35<\/td>\n<td>0.15<\/td>\n<td>0.01 &#8211; 0.1<\/td>\n<\/tr>\n<tr>\n<th>Depth of cut mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.01 &#8211; 0.1<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Turning in annealed conditions<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Carbide insert<br \/>Rough turning<\/th>\n<th>Carbide insert<br \/>\u00bd Finishing<\/th>\n<th>HSS tool<br \/>Turning<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>110 &#8211; 140<\/td>\n<td>165 &#8211; 200<\/td>\n<td>15<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/r<\/th>\n<td>0.35<\/td>\n<td>0.15<\/td>\n<td>0.1- 0.2<\/td>\n<\/tr>\n<tr>\n<th>Depth of cut mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.5 &#8211; 2.0<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Drilling in annealed conditions<br \/>Carbide drill<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Insert<\/th>\n<th>Solid<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Cutting speed m\/min<\/th>\n<td>130<\/td>\n<td>70<\/td>\n<\/tr>\n<tr>\n<th>Feed mm\/r<\/th>\n<td>0.10<\/td>\n<td>0.20<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>HSS twist drill<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Drill diameter mm<\/th>\n<th>Cutting speed m\/min<\/th>\n<th>Feed mm\/r<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>&lt; 5<\/td>\n<td rowspan=\"4\">11<\/td>\n<td>0.07<\/td>\n<\/tr>\n<tr>\n<td>5 &#8211; 10<\/td>\n<td>0.15<\/td>\n<\/tr>\n<tr>\n<td>10 &#8211; 15<\/td>\n<td>0.22<\/td>\n<\/tr>\n<tr>\n<td>15 &#8211; 20<\/td>\n<td>0.30<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Fine grinding<\/h4>\n<p>General indications for grinding wheels to be used on TPM23 UltraClean in the heat treated condition.<\/p>\n<p>Usually, rather soft vitrified aluminum oxide grinding wheels <em>(grades G for plane grinding to K for cylindrical grinding)<\/em> are used.<\/p>\n<p>Particular attention will be paid to effective cooling of the surface during grinding to prevent degradation of the material surface.<\/p>\n<h4>Electro-discharge machining<\/h4>\n<p>TPM23 UltraClean is also suitable for EDM machining <em>(wire or electrode)<\/em>. Preferably, the machining will be carried out with a low current density and a high frequency in order to limit the thickness of the white layer as much as possible.<\/p>\n<p>Then it is necessary to carry out a stress relieving at 25\u00b0C below the last tempering in order to reduce the level of residual stresses <em>(which could lead to a risk of cracking)<\/em> and to carry out a polishing to completely remove the white layer formed during the discharge machining process.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=&#8221;in_container&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; scene_position=&#8221;center&#8221; bottom_padding=&#8221;120&#8243; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221; column_element_direction_desktop=&#8221;default&#8221; column_element_spacing=&#8221;default&#8221; desktop_text_alignment=&#8221;default&#8221; tablet_text_alignment=&#8221;default&#8221; phone_text_alignment=&#8221;default&#8221; background_color_opacity=&#8221;1&#8243; background_hover_color_opacity=&#8221;1&#8243; column_backdrop_filter=&#8221;none&#8221; column_shadow=&#8221;none&#8221; column_border_radius=&#8221;none&#8221; column_link_target=&#8221;_self&#8221; column_position=&#8221;default&#8221; gradient_direction=&#8221;left_to_right&#8221; overlay_strength=&#8221;0.3&#8243; width=&#8221;1\/1&#8243; tablet_width_inherit=&#8221;default&#8221; animation_type=&#8221;default&#8221; bg_image_animation=&#8221;none&#8221; border_type=&#8221;simple&#8221; column_border_width=&#8221;none&#8221; column_border_style=&#8221;solid&#8221;][vc_column_text css=&#8221;&#8221; text_direction=&#8221;default&#8221;]\n<div style=\"max-width:680px\">\n<p><a href=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/02\/TPM23-Ultraclean.pdf\" target=\"_blank\" rel=\"noopener\"><strong>Download the TPM 23 Ultraclean datasheet (PDF)<\/strong><\/a><\/p>\n<p>More grades: <a href=\"https:\/\/www.tgsteels.com\/en\/cold-work-tool-steels\/\">Cold Work Tool Steels<\/a>. Where to buy: <a href=\"https:\/\/www.tgsteels.com\/en\/service-network\/\">Service Network<\/a>.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row]\n","protected":false},"excerpt":{"rendered":"<p>[vc_row type=&#8221;full_width_background&#8221; full_screen_row_position=&#8221;middle&#8221; column_margin=&#8221;default&#8221; column_direction=&#8221;default&#8221; column_direction_tablet=&#8221;default&#8221; column_direction_phone=&#8221;default&#8221; video_bg=&#8221;use_video&#8221; video_mp4=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&#8243; video_webm=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm&#8221; video_ogv=&#8221;https:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv&#8221; background_video_loading=&#8221;default&#8221; scene_position=&#8221;center&#8221; text_color=&#8221;dark&#8221; text_align=&#8221;left&#8221; row_border_radius=&#8221;none&#8221; row_border_radius_applies=&#8221;bg&#8221; overflow=&#8221;visible&#8221; overlay_strength=&#8221;0.3&#8243; gradient_direction=&#8221;left_to_right&#8221; shape_divider_position=&#8221;bottom&#8221; bg_image_animation=&#8221;none&#8221; parallax_bg=&#8221;true&#8221; parallax_bg_speed=&#8221;fast&#8221; gradient_type=&#8221;default&#8221; shape_type=&#8221;&#8221;][vc_column column_padding=&#8221;no-extra-padding&#8221; column_padding_tablet=&#8221;inherit&#8221; column_padding_phone=&#8221;inherit&#8221; column_padding_position=&#8221;all&#8221;&#8230;<\/p>\n","protected":false},"author":6,"featured_media":0,"parent":546,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"inline_featured_image":false,"footnotes":""},"class_list":["post-4080","page","type-page","status-publish"],"_links":{"self":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4080","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/comments?post=4080"}],"version-history":[{"count":3,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4080\/revisions"}],"predecessor-version":[{"id":5141,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/4080\/revisions\/5141"}],"up":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/pages\/546"}],"wp:attachment":[{"href":"https:\/\/www.tgsteels.com\/en\/wp-json\/wp\/v2\/media?parent=4080"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}