{"id":4523,"date":"2026-10-08T14:32:00","date_gmt":"2026-10-08T14:32:00","guid":{"rendered":"https:\/\/www.tgsteels.com\/?page_id=4523"},"modified":"2026-10-29T10:04:55","modified_gmt":"2026-10-29T10:04:55","slug":"tpm-4v-ultraclean","status":"publish","type":"page","link":"https:\/\/www.tgsteels.com\/fr\/aciers-de-travail-a-froid\/tpm-4v-ultraclean\/","title":{"rendered":"TPM 4V Ultraclean"},"content":{"rendered":"[vc_row type=\u00a0\u00bbfull_width_background\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb video_bg=\u00a0\u00bbuse_video\u00a0\u00bb video_mp4=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&Prime; video_webm=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm\u00a0\u00bb video_ogv=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv\u00a0\u00bb background_video_loading=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb parallax_bg=\u00a0\u00bbtrue\u00a0\u00bb parallax_bg_speed=\u00a0\u00bbfast\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/2&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb column_padding_type=\u00a0\u00bbdefault\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb][divider line_type=\u00a0\u00bbNo Line\u00a0\u00bb custom_height=\u00a0\u00bb450&Prime;][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<h1>TPM 4V Ultraclean<\/h1>\n[\/vc_column_text][divider line_type=\u00a0\u00bbNo Line\u00a0\u00bb custom_height=\u00a0\u00bb50&Prime;][\/vc_column][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/2&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h4>Acier \u00e9labor\u00e9 par m\u00e9tallurgie des poudres pour une bonne r\u00e9sistance \u00e0 l\u2019usure et une bonne t\u00e9nacit\u00e9<\/h4>\n<\/div>\n[\/vc_column_text][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<p>L\u2019acier \u00e0 outils TPM4V ULTRACLEAN est \u00e9labor\u00e9 par m\u00e9tallurgie des poudres. Il se caract\u00e9rise par une tr\u00e8s bonne t\u00e9nacit\u00e9 associ\u00e9e \u00e0 une tr\u00e8s bonne r\u00e9sistance \u00e0 l\u2019usure.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Applications<\/h3>\n<p>TPM4V ULTRACLEAN trouve de nombreuses applications dans le domaine des outils de travail \u00e0 froid, n\u00e9cessitant soit une bonne t\u00e9nacit\u00e9 ainsi qu\u2019une bonne r\u00e9sistance \u00e0 l\u2019usure, comme les outils de d\u00e9coupe fine, ainsi que pour les poin\u00e7ons ou les matrices <em>(outils d\u2019emboutissage profond)<\/em>, les outils de compression de poudres, les couteaux pour mat\u00e9riaux tendres&#8230;.<\/p>\n<p>TPM4V ULTRACLEAN est particuli\u00e8rement recommand\u00e9 pour les outils o\u00f9 l\u2019usure ou l\u2019\u00e9caillage sont les principaux m\u00e9canismes de d\u00e9faillance, comme par exemple les outils utilis\u00e9s dans la transformation de m\u00e9taux tendres tels que l\u2019aluminium ou le cuivre.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Propri\u00e9t\u00e9s principales<\/h3>\n<ul>\n<li>Bonne t\u00e9nacit\u00e9 associ\u00e9e \u00e0 une bonne r\u00e9sistance \u00e0 l\u2019usure<\/li>\n<li>Tr\u00e8s bonne r\u00e9sistance \u00e0 la compression<\/li>\n<li>Tr\u00e8s bonne stabilit\u00e9<\/li>\n<\/ul>\n<p>La comparaison avec les autres aciers \u00e0 outils \u00e9labor\u00e9s en m\u00e9tallurgie des poudres disponibles chez TG Steels est indiqu\u00e9e sur le diagramme tenacit\u00e9 vs usure  pr\u00e9sent\u00e9 ci-dessous.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Composition chimique <em>(typique)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>C<\/th>\n<th>W<\/th>\n<th>Mo<\/th>\n<th>Cr<\/th>\n<th>V<\/th>\n<th>Co<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1.40<\/td>\n<td>&#8211;<\/td>\n<td>3.,50<\/td>\n<td>4.70<\/td>\n<td>3.70<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h3>D\u00e9signation<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Nuance<\/th>\n<th>ISO<\/th>\n<th>Chine GB<\/th>\n<th>JIS Japon<\/th>\n<th>UK<\/th>\n<th>AISI USA<\/th>\n<th>Russie Gost<\/th>\n<th>AFNOR<\/th>\n<th>Autres \/ Sp\u00e9cial<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>&#8211;<\/td>\n<td>X140CrVMo 5-4-3<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<td>&#8211;<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p><img decoding=\"async\" class=\"wp-image-4468\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure.png\" alt=\"TPM 4V Ultraclean, diagramme de positionnement des aciers PM disponibles chez TG Steels : t\u00e9nacit\u00e9 (axe vertical) en fonction de la r\u00e9sistance \u00e0 l\u2019usure (axe horizontal), TPM 4V \u00e0 r\u00e9sistance \u00e0 l\u2019usure moyenne et t\u00e9nacit\u00e9 sup\u00e9rieure \u00e0 la moyenne, pr\u00e8s de TPM 39 et TPM 23\" width=\"1016\" height=\"411\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure.png 1538w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure-300x121.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure-1024x414.png 1024w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure-768x311.png 768w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-diagramme-tenacite-usure-1536x621.png 1536w\" sizes=\"auto, (max-width: 1016px) 100vw, 1016px\" \/><\/p>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Structure<\/h3>\n<p>La structure du TPM4V ULTRACLEAN est fine et homog\u00e8ne, sans pr\u00e9cipitations ni alignements de carbures.<\/p>\n<p>Gr\u00e2ce \u00e0 son \u00e9laboration par m\u00e9tallurgie des poudres avec compression isostatique \u00e0 chaud, la taille typique des carbures est d\u2019environ 2 \u03bcm et le niveau de propret\u00e9 est bien meilleur que celui des aciers \u00e0 outils \u00e0 froid conventionnels.<\/p>\n<h3>Duret\u00e9 \u00e0 l\u2019\u00e9tat de livraison<\/h3>\n<p>Recuit pour 310 HB max.<\/p>\n<h3>Propri\u00e9t\u00e9s m\u00e9caniques typiques \u00e0 l\u2019\u00e9tat trait\u00e9 <em>(r\u00e9sultats d\u2019essais internes non indiqu\u00e9s sur les certificats)<\/em><\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Duret\u00e9<\/th>\n<th>Limite \u00e9lastique \u00e0 la compression MPa<\/th>\n<th>R\u00e9silience eprouvette non entaill\u00e9e J \u00e0 23\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>58<\/td>\n<td>3200<\/td>\n<td>75<\/td>\n<\/tr>\n<tr>\n<td>60<\/td>\n<td>3800<\/td>\n<td>70<\/td>\n<\/tr>\n<tr>\n<td>62<\/td>\n<td>4000<\/td>\n<td>65<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Propri\u00e9t\u00e9s physiques<\/h3>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Temp\u00e9rature<\/th>\n<th>20\u00b0C<\/th>\n<th>400\u00b0C<\/th>\n<th>600\u00b0C<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Masse Volumique kg\/m<sup>3<\/sup><\/th>\n<td>7700<\/td>\n<td>7500<\/td>\n<td>7350<\/td>\n<\/tr>\n<tr>\n<th>Module d\u2019Young N\/mm\u00b2<\/th>\n<td>206000<\/td>\n<td>200000<\/td>\n<td>180000<\/td>\n<\/tr>\n<tr>\n<th>Conductivit\u00e9 thermique W\/m.K<\/th>\n<td>28<\/td>\n<td>30<\/td>\n<td>31<\/td>\n<\/tr>\n<tr>\n<th>Coefficient de dilatation lin\u00e9aire10<sup>-6<\/sup>\/K<\/th>\n<td>11<\/td>\n<td>11.5<\/td>\n<td>12.2<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Traitement thermique<\/h3>\n<h4>Recuit d\u2019adoucissement<\/h4>\n<p>Temp\u00e9rature: 870 &#8211; 890\u00b0C, dur\u00e9e 1h + 1h pour une \u00e9paisseur de 25 mm. Refroidissement lent au four <em>(10 \u00e0 20\u00b0C \/ h)<\/em>. L\u2019atmosph\u00e8re dans le four doit \u00eatre r\u00e9ductrice pour \u00e9viter la d\u00e9carburation de l\u2019acier.<\/p>\n<h4>Detentionnement<\/h4>\n<p>Apr\u00e8s l\u2019usinage, il est recommand\u00e9 d\u2019effectuer un d\u00e9tensionnement \u00e0 650\u00b0C pendant au moins 2 heures, suivi d\u2019un refroidissement lent dans le four jusqu\u2019\u00e0 450\u00b0C.<\/p>\n<h4>Austenitization<\/h4>\n<p>Pour \u00e9viter tout risque de fissure, il est recommand\u00e9 de pr\u00e9chauffer en 2 \u00e9tapes.<\/p>\n<ul>\n<li>1re \u00e9tape de pr\u00e9chauffage: temp\u00e9rature: 600\u00b0C Dur\u00e9e: 30 s\/mm d\u2019\u00e9paisseur<\/li>\n<li>2e \u00e9tape de pr\u00e9chauffage: temp\u00e9rature: 875\u00b0C Dur\u00e9e: 30 s\/mm d\u2019\u00e9paisseur<\/li>\n<\/ul>\n<p>Temp\u00e9rature d\u2019austenitisation recommand\u00e9e: 1010 &#8211; 1020\u00b0C. Le temps de maintien ne doit pas \u00eatre trop long pour \u00e9viter un risque de grossissement du grain et de perte de t\u00e9nacit\u00e9. Il est recommand\u00e9 de maintenir la pi\u00e8ce \u00e0 la temp\u00e9rature d\u2019austenitisation: 30 minutes par pouce d\u2019\u00e9paisseur d\u00e8s que la temp\u00e9rature de surface atteint la temp\u00e9rature d\u2019aust\u00e9nitisation. Des temp\u00e9ratures sup\u00e9rieures \u00e0 1020\u00b0C ne sont pas recommand\u00e9es afin d\u2019\u00e9viter de grandes quantit\u00e9s d\u2019aust\u00e9nite r\u00e9siduelle, ce qui entra\u00eene une mauvaise stabilit\u00e9 et un risque de fissures.<\/p>\n<h4>Milieu de trempe<\/h4>\n<p>Huile \u00e0 80\u00b0C, vide <em>(pression &gt; 6 bars)<\/em>, bain de sel 500 &#8211; 550\u00b0C.<br \/>\nPour garantir une bonne t\u00e9nacit\u00e9, il est pr\u00e9f\u00e9rable de traiter \u00e0 l\u2019huile ou en bain de sel.<\/p>\n<h4>Traitement par le froid<\/h4>\n<p>Pour les pi\u00e8ces qui doivent avoir une grande stabilit\u00e9 dimensionnelle et augmenter la r\u00e9sistance \u00e0 l\u2019usure sans r\u00e9duire la t\u00e9nacit\u00e9, il est recommand\u00e9 de r\u00e9aliser un traitement par le froid \u00e0 une temp\u00e9rature comprise entre -70\u00b0C et -190\u00b0C pendant 1 heure pour 25 mm d\u2019\u00e9paisseur de la pi\u00e8ce. La plage de temp\u00e9rature allant de -70\u00b0C \u00e0 -120\u00b0C <em>(appel\u00e9 traitement \u00e0 froid de l\u2019acier)<\/em> conduit \u00e0 la transformation compl\u00e8te de l\u2019aust\u00e9nite en martensite et, par cons\u00e9quent, \u00e0 une meilleure stabilit\u00e9 associ\u00e9e \u00e0 une duret\u00e9 am\u00e9lior\u00e9e et une meilleure r\u00e9sistance \u00e0 l\u2019usure et la plage de temp\u00e9rature de -135\u00b0C jusqu\u2019\u00e0 -190\u00b0C <em>(appel\u00e9 cryotraitement de l\u2019acier)<\/em> conduit \u00e9galement \u00e0 la transformation compl\u00e8te de l\u2019aust\u00e9nite et \u00e0 la pr\u00e9cipitation de carbures ultrafins, am\u00e9liorant consid\u00e9rablement la r\u00e9sistance \u00e0 l\u2019usure sans modification de la t\u00e9nacit\u00e9. Ce traitement est optionnel pour les applications courantes.<\/p>\n<h4>Revenu<\/h4>\n<p>Pour garantir un taux d\u2019aust\u00e9nite r\u00e9siduelle minimal ainsi qu\u2019une meilleure stabilit\u00e9 de l\u2019outil, il est essentiel de r\u00e9aliser un double <em>(meilleur triple)<\/em> revenu. Chaque revenu est suivi d\u2019un refroidissement \u00e0 temp\u00e9rature inf\u00e9rieure \u00e0 100\u00b0C. Selon l\u2019utilisation de la pi\u00e8ce, les temp\u00e9ratures de revenu suivantes sont recommand\u00e9es:<\/p>\n<\/div>\n[\/vc_column_text]\n<table>\n<thead>\n<tr>\n<th>Temp\u00e9rature d\u2019austenitisation<\/th>\n<th>Temp\u00e9rature de revenu<\/th>\n<th>Duret\u00e9<\/th>\n<th>Propri\u00e9t\u00e9s<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td rowspan=\"3\">1010 \/ 1020\u00b0C<\/td>\n<td>530\u00b0C<\/td>\n<td>60 \/ 62 HRC<\/td>\n<td>Meilleure r\u00e9sistance \u00e0 l\u2019usure<\/td>\n<\/tr>\n<tr>\n<td>550\u00b0C<\/td>\n<td>57 \/ 59 HRC<\/td>\n<td>R\u00e9sisttance \u00e0 l\u2019usure et t\u00e9nacit\u00e9<\/td>\n<\/tr>\n<tr>\n<td>560\u00b0C<\/td>\n<td>56 \/ 58 HRC<\/td>\n<td>meilleure t\u00e9nacit\u00e9<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<p>* \u00c9vitez de faire un revenu en dessous de 520\u00b0C et de pr\u00e9f\u00e9rence au-dessus de 540\u00b0C.<\/p>\n<p>Chaque dur\u00e9e de revenu doit \u00eatre au moins \u00e9gale \u00e0 1h + 1h pour 25 mm d\u2019\u00e9paisseur de la pi\u00e8ce trait\u00e9e <em>(\u00e9paisseur thermique \u00e9quivalente)<\/em>.<\/p>\n<\/div>\n[\/vc_column_text][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<p><img decoding=\"async\" class=\"wp-image-4469\" src=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu.png\" alt=\"TPM 4V Ultraclean, courbe de revenu : duret\u00e9 (HRC) en fonction de la temp\u00e9rature de revenu (400 \u00e0 600 \u00b0C) apr\u00e8s aust\u00e9nitisation \u00e0 940, 980 et 1020 \u00b0C, avec l\u2019aust\u00e9nite r\u00e9siduelle (%) pour 1020 \u00b0C en pointill\u00e9s\" width=\"520\" height=\"516\" loading=\"lazy\" style=\"max-width:100%;height:auto\" srcset=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu.png 688w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu-300x298.png 300w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu-150x150.png 150w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu-140x140.png 140w, https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/10\/tpm-4v-ultraclean-courbe-de-revenu-100x100.png 100w\" sizes=\"auto, (max-width: 520px) 100vw, 520px\" \/><\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Traitement de surface<\/h3>\n<h4>Nitruration<\/h4>\n<p>Le TPM4V ULTRACLEAN peut \u00eatre nitrur\u00e9 \u00e0 des temp\u00e9ratures inf\u00e9rieures ou \u00e9gales \u00e0 20\u00b0C sous les temp\u00e9ratures de revenu sans risque de d\u00e9t\u00e9rioration des caract\u00e9ristiques m\u00e9caniques. La nitruration ionique \u00e0 une temp\u00e9rature de 500\u00b0C est recommand\u00e9e. La duret\u00e9 de surface apr\u00e8s nitruration est d\u2019environ 1200 HV<sub>0.2kg<\/sub>.<\/p>\n<h4>PVD, CVD<\/h4>\n<p>TPM4V ULTRACLEAN convient \u00e0 tous types de traitements PVD et CVD d\u00e8s que la temp\u00e9rature de traitement est inf\u00e9rieure de 30\u00b0C \u00e0 la derni\u00e8re temp\u00e9rature de revenu.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb60&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h3>Usinage<\/h3>\n<p>Les param\u00e8tres d\u2019usinage ci-dessous sont donn\u00e9s uniquement pour l\u2019information et doivent \u00eatre adapt\u00e9s en fonction de l\u2019\u00e9quipement et des conditions habituelles d\u2019usinage.<\/p>\n<h4>Fraisage surfa\u00e7age \u00e0 l\u2019\u00e9tat recuit<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th colspan=\"2\">Outils carbure<\/th>\n<th>Outils rapide<\/th>\n<\/tr>\n<tr>\n<th><\/th>\n<th>\u00c9bauchage<\/th>\n<th>\u00bd Finition<\/th>\n<th>Finition<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Vitesse de coupe m\/min<\/th>\n<td>120 &#8211; 140<\/td>\n<td>160 &#8211; 190<\/td>\n<td>60 &#8211; 70<\/td>\n<\/tr>\n<tr>\n<th>Avance mm\/r<\/th>\n<td>0.35<\/td>\n<td>0.15<\/td>\n<td>0.05 &#8211; 0.15<\/td>\n<\/tr>\n<tr>\n<th>Profondeur de coupe mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.01 &#8211; 0.1<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n[\/vc_column_text][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<h4>Tournage \u00e0 l\u2019\u00e9tat recuit<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th colspan=\"2\">Outils carbure<\/th>\n<th>Monobloc<\/th>\n<\/tr>\n<tr>\n<th><\/th>\n<th>\u00c9bauchage<\/th>\n<th>\u00bd Finition<\/th>\n<th>Finition<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Vitesse de coupe m\/min<\/th>\n<td>120 &#8211; 150<\/td>\n<td>180 &#8211; 210<\/td>\n<td>17<\/td>\n<\/tr>\n<tr>\n<th>Avance mm\/r<\/th>\n<td>0.350<\/td>\n<td>0.15<\/td>\n<td>0.1 &#8211; 0.2<\/td>\n<\/tr>\n<tr>\n<th>Profondeur de coupe mm<\/th>\n<td>2 &#8211; 3<\/td>\n<td>1 &#8211; 1.5<\/td>\n<td>0.5 &#8211; 2.0<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Per\u00e7age \u00e0 l\u2019\u00e9tat recuit outils carbure<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th><\/th>\n<th>Insert<\/th>\n<th>Monobloc<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<th>Vitesse de coupe m\/min<\/th>\n<td>150<\/td>\n<td>90<\/td>\n<\/tr>\n<tr>\n<th>Avance mm\/r<\/th>\n<td>0.10<\/td>\n<td>0.15<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Per\u00e7age a l\u2019etat recuit: for\u00eat h\u00e9licoidal en acier rapide<\/h4>\n<\/div>\n<table>\n<thead>\n<tr>\n<th>Diametre du for\u00eat mm<\/th>\n<th>Vitesse de coupe m\/min<\/th>\n<th>Avance mm\/t<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>&lt; 5<\/td>\n<td rowspan=\"4\">13<\/td>\n<td>0.10<\/td>\n<\/tr>\n<tr>\n<td>5 &#8211; 10<\/td>\n<td>0.17<\/td>\n<\/tr>\n<tr>\n<td>10 &#8211; 15<\/td>\n<td>0.22<\/td>\n<\/tr>\n<tr>\n<td>15 &#8211; 20<\/td>\n<td>0.30<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<div style=\"max-width:680px\">\n<h4>Rectification<\/h4>\n<p>Indications g\u00e9n\u00e9rales pour l\u2019utilisation de meules de rectification sur TPM4V ULTRACLEAN \u00e0 l\u2019\u00e9tat trait\u00e9. En g\u00e9n\u00e9ral, on utilise des meules \u00e0 l\u2019oxyde d\u2019aluminium vitrifi\u00e9 assez tendres <em>(grades G \u00e0 K pour la rectification cylindrique)<\/em>.<\/p>\n<p>Une attention particuli\u00e8re sera port\u00e9e au refroidissement efficace de la surface lors du meulage afin d\u2019\u00e9viter la d\u00e9gradation de la surface de la pi\u00e8ce.<\/p>\n<h4>Usinage par \u00e9lectroerosion<\/h4>\n<p>TPM4V ULTRACLEAN convient \u00e9galement \u00e0 l\u2019usinage par \u00e9lectro\u00e9rosion <em>(fil ou \u00e9lectrode)<\/em>. De pr\u00e9f\u00e9rence, l\u2019usinage sera effectu\u00e9 avec une faible densit\u00e9 de courant et une fr\u00e9quence \u00e9lev\u00e9e afin de limiter au maximum l\u2019\u00e9paisseur de la couche blanche.<\/p>\n<p>Il est ensuite n\u00e9cessaire de r\u00e9aliser un d\u00e9tensionnement \u00e0 25\u00b0C en dessous du dernier revenu afin de r\u00e9duire le niveau de contraintes r\u00e9siduelles <em>(qui pourraient entra\u00eener un risque de fissure)<\/em> et effectuer un polissage pour \u00e9liminer compl\u00e8tement la couche blanche form\u00e9e lors du processus d\u2019usinage par \u00e9lectro\u00e9rosion.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row][vc_row type=\u00a0\u00bbin_container\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb bottom_padding=\u00a0\u00bb120&Prime; text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb column_element_direction_desktop=\u00a0\u00bbdefault\u00a0\u00bb column_element_spacing=\u00a0\u00bbdefault\u00a0\u00bb desktop_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb tablet_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb phone_text_alignment=\u00a0\u00bbdefault\u00a0\u00bb background_color_opacity=\u00a0\u00bb1&Prime; background_hover_color_opacity=\u00a0\u00bb1&Prime; column_backdrop_filter=\u00a0\u00bbnone\u00a0\u00bb column_shadow=\u00a0\u00bbnone\u00a0\u00bb column_border_radius=\u00a0\u00bbnone\u00a0\u00bb column_link_target=\u00a0\u00bb_self\u00a0\u00bb column_position=\u00a0\u00bbdefault\u00a0\u00bb gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; width=\u00a0\u00bb1\/1&Prime; tablet_width_inherit=\u00a0\u00bbdefault\u00a0\u00bb animation_type=\u00a0\u00bbdefault\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb border_type=\u00a0\u00bbsimple\u00a0\u00bb column_border_width=\u00a0\u00bbnone\u00a0\u00bb column_border_style=\u00a0\u00bbsolid\u00a0\u00bb][vc_column_text css=\u00a0\u00bb\u00a0\u00bb text_direction=\u00a0\u00bbdefault\u00a0\u00bb]\n<div style=\"max-width:680px\">\n<p><a href=\"https:\/\/www.tgsteels.com\/wp-content\/uploads\/2026\/05\/TPM4V-Ultraclean-FR.pdf\" target=\"_blank\" rel=\"noopener\"><strong>T\u00e9l\u00e9charger la fiche technique TPM 4V Ultraclean (PDF)<\/strong><\/a><\/p>\n<p>Autres nuances&nbsp;: <a href=\"https:\/\/www.tgsteels.com\/fr\/aciers-de-travail-a-froid\/\">Aciers de Travail \u00e0 Froid<\/a>. O\u00f9 acheter&nbsp;: <a href=\"https:\/\/www.tgsteels.com\/fr\/reseau-de-services\/\">R\u00e9seau de Services<\/a>.<\/p>\n<\/div>\n[\/vc_column_text][\/vc_column][\/vc_row]\n","protected":false},"excerpt":{"rendered":"<p>[vc_row type=\u00a0\u00bbfull_width_background\u00a0\u00bb full_screen_row_position=\u00a0\u00bbmiddle\u00a0\u00bb column_margin=\u00a0\u00bbdefault\u00a0\u00bb column_direction=\u00a0\u00bbdefault\u00a0\u00bb column_direction_tablet=\u00a0\u00bbdefault\u00a0\u00bb column_direction_phone=\u00a0\u00bbdefault\u00a0\u00bb video_bg=\u00a0\u00bbuse_video\u00a0\u00bb video_mp4=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.mp4&Prime; video_webm=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.webm\u00a0\u00bb video_ogv=\u00a0\u00bbhttps:\/\/www.tgsteels.com\/wp-content\/uploads\/2025\/09\/hss-hero-1.ogv\u00a0\u00bb background_video_loading=\u00a0\u00bbdefault\u00a0\u00bb scene_position=\u00a0\u00bbcenter\u00a0\u00bb text_color=\u00a0\u00bbdark\u00a0\u00bb text_align=\u00a0\u00bbleft\u00a0\u00bb row_border_radius=\u00a0\u00bbnone\u00a0\u00bb row_border_radius_applies=\u00a0\u00bbbg\u00a0\u00bb overflow=\u00a0\u00bbvisible\u00a0\u00bb overlay_strength=\u00a0\u00bb0.3&Prime; gradient_direction=\u00a0\u00bbleft_to_right\u00a0\u00bb shape_divider_position=\u00a0\u00bbbottom\u00a0\u00bb bg_image_animation=\u00a0\u00bbnone\u00a0\u00bb parallax_bg=\u00a0\u00bbtrue\u00a0\u00bb parallax_bg_speed=\u00a0\u00bbfast\u00a0\u00bb gradient_type=\u00a0\u00bbdefault\u00a0\u00bb shape_type=\u00a0\u00bb\u00a0\u00bb][vc_column column_padding=\u00a0\u00bbno-extra-padding\u00a0\u00bb column_padding_tablet=\u00a0\u00bbinherit\u00a0\u00bb column_padding_phone=\u00a0\u00bbinherit\u00a0\u00bb column_padding_position=\u00a0\u00bball\u00a0\u00bb&#8230;<\/p>\n","protected":false},"author":6,"featured_media":0,"parent":1235,"menu_order":0,"comment_status":"closed","ping_status":"closed","template":"","meta":{"inline_featured_image":false,"footnotes":""},"class_list":["post-4523","page","type-page","status-publish"],"_links":{"self":[{"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/pages\/4523","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/pages"}],"about":[{"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/types\/page"}],"author":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/users\/6"}],"replies":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/comments?post=4523"}],"version-history":[{"count":3,"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/pages\/4523\/revisions"}],"predecessor-version":[{"id":5225,"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/pages\/4523\/revisions\/5225"}],"up":[{"embeddable":true,"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/pages\/1235"}],"wp:attachment":[{"href":"https:\/\/www.tgsteels.com\/fr\/wp-json\/wp\/v2\/media?parent=4523"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}