Skip to main content

CROMIS ESR

Stainless mold steel for either good corrosion resistance and high mechanical properties with the highest polishability

CROMIS ESR is Electroslag Remelted (ESR) stainless steel, which can be used for making small and medium-sized plastic injection molds where a good corrosion resistance is required with a mirror polishing level.

Applications

CROMIS ESR has both very high wear resistance, excellent corrosion resistance, excellent polishability ((suitable for applications requiring a mirror polished level) as well as correct machinability.

CROMIS ESR can be used for injection molds for corrosive plastic (PVC, recycled plastics…), molds for plastics reinforced with abrasive fillers, extrusion screws and barrels for extruders, molds for food, medical and optical equipment and for all the molds requiring a mirror polish.

CROMIS ESR is delivered in the annealed condition and in use it should be treated to a hardness of 52 HRC.

Main properties

  • Good corrosion resistance
  • Very good polishability
  • Good wear resistance
  • High hardenabilty

Chemical composition (typical)

C Mn Si P S Cr Mo
0.40 0.30 Max 0.3 < 0.015 < 0.005 14.0 0.20

Designation

Werkstoff Nr ISO China GB JIS Japan UK AISI USA Russia Gost AFNOR Other / Special
1.2083 ESR X42Cr13 4Cr13 SUS420J2 420S45 420 ESR 40KH13 Z40C13 –

Structure

The structure of the CROMIS ESR is fine and homogeneous without precipitation or alignments of carbides.

The cleanliness of CROMIS ESR which is a electroslag remelted steel (ESR) is very high and according to ASTM E 45-95 method A it is at most equal to: fine series: A0.5 – B0.5 – C0 – D1.5 / thick: A0.5 – B0.5 – C0-D1 and B + C + D less than 2.5. This level of cleanliness guarantees the highest polishability of CROMIS ESR.

Hardness at the time of delivery

Annealed for 230 HB max.

Typical mechanical properties in hardened conditions (results from internal tests not indicated on the certificates)

TS MPa YS 0.2% MPa Elongation % Hardness HRC KU J à 20°C
≥ 1700 ≥ 1300 ≥ 12 ≥ 50 ≥ 18

Physical properties

Temperature 20°C 200°C 400°C
Volumic mass kg/m³ 7800 7750 7700
Young Modulus N/mm² 215000 202000 190000
Thermal conductivity W/m.K 22 24 27
Coefficient of linear expansion 10-6/K 10.5 10.9 11.5

Heat treatment

Soft annealing

Temperature: 760 – 790°C, duration 1h + 1h for 25 mm thickness. Slow cooling in the furnace (10 to 20°C/h). The atmosphere in the furnace must be reducing to avoid decarburization of the steel.

Stress relieving

After machining, it is recommended to perform stress relieving at 650°C for a minimum of 2 hours, followed by slow cooling in the furnace to 450°C.

Austenitization

In order to avoid any risk of cracking it is recommended to preheat in 2 steps.

  • 1st preheating step: temperature: 600°C time: 30 s/mm of thickness
  • 2nd preheating step: temperature: 850°C time: 30 s/mm of thickness

Recommended austenitizing temperature: 1000 – 1050°C. The holding time should not be too long to avoid a risk of grain coarsening and a loss of toughness. It is recommended to keep the part at the austenitizing temperature 30 minutes per inch of thickness as soon as the temperature of the surface reach the austenitization temperature.

Quenching medium

Oil at 80°C, vacuum (pressure > 6 Bars), salt bath 500 – 550°C.
To ensure good toughness, treatment with oil or salt bath is preferable.

Tempering

To ensure a minimum residual austenite rate as well as greater tool stability, it is essential to perform a double tempering. Each tempering is followed by a cooling under 100°C.

Each tempering time must be at least equal to 1h + 1h for 25 mm of thickness of the treated part (equivalent thermal thickness).

Tempering temperature and corrosion resistance: In order to avoid a better corrosion resistance it is highly recommended to avoid tempering temperatures in the range 400 to 550°C since at these temperatures there is a precipitation of chromium carbides at the grain boundaries leading to an increase of the local corrosion at these locations.

For the higher hardness (better wear resistance) tempering temperatures lower than 400°C are recommended and for lower hardness (better toughness) tempering temperatures over 550°C are recommended.

CROMIS ESR tempering curve: hardness (HRC) versus tempering temperature (0 to 800 °C), about 56 HRC up to 150 °C, a minimum near 51 HRC at 400 °C, a secondary maximum near 52 HRC at 500 °C and a sharp drop to about 40 HRC at 600 °C

Surface treatment

Nitriding

CROMIS ESR can be nitrided at temperatures less than or equal to 20°C below tempering temperatures without risk of deterioration of the mechanical characteristics. Nitriding at a temperature over 550°C is recommended to avoid any risk of carbide precipitation at the grain boundaries.

PVD, CVD

CROMIS ESR is suitable for all kind of PVD and CVD treatment as soon as the treatment temperature is 30°C lower than the last tempering temperature.

Polishing

CROMIS ESR is suitable for polishing in the heat treated condition and it can be used for applications requiring a mirror polished level (Rt ≤ 0.25 µm, CNOMO level 1, Rugotest N1).

Optimal polishing is achieved by performing consecutive steps with similar roughness and stopping each step as soon as the last scratch from the previous step disappears.

Texturing

CROMIS ESR is suitable for chemical or laser texturing.

Machining

The machining parameters below are given for information only and must be adapted according to the equipment and usual machining conditions.

Turning

Carbide tool
Rough machining
Carbide tool
Finishing
HSS tool
Finishing
Cutting speed m/min 160 – 200 210 – 250 17 – 22
Feed mm/r 0.2 – 0.4 0.1 – 0.2 0.1 – 0.3
Depth of cut mm 2 – 4 0.5 – 2 0.5 – 2

Milling: surfacing

Milling with carbide tools
Rough machining
Milling with carbide tools
Finishing
Cutting speed m/ min 160 – 200 250 – 280
Feed mm/r 0.2 – 0.4 0.1 – 0.2
Depth of cut mm 2 – 4 0.5 – 2
Carbide designation ISO P20 – P40 coated carbide P10 – P20 coated carbide or cermet

End milling

Milling with carbide tools
Solid carbide
Milling with carbide tools
Carbide indexable insert
HSS milling tool
Cutting speed m/ min 120 – 150 160 – 210 25 – 29
Feed mm/teeth 0.02 – 0.2 0.07 – 0.2 0.01 – 0.3
Carbide designation ISO NA P20 – P30 NA

Drilling: HSS twist drill

Drill diameter mm Cutting speed m/min Feed mm/t
< 5 14 – 16 0.05 – 0.15
5 – 10 14 – 16 0.15 – 0.20
10 – 15 14 – 16 0.20 – 0.25
15 – 20 14 – 16 0.25 – 0.30

Drilling: carbide drill

Carbide type Indexable insert Solid carbid Carbide tip
Cutting speed m/ min 210 – 230 80 – 100 70 – 80
Feed mm/t 0.05 – 0.10 0.10 – 0.25 0.15 – 0.25

Fine grinding

General indications for grinding wheels to be used on CROMIS ESR in the heat treated condition. Usually, rather soft vitrified aluminum oxide grinding wheels (grades G for plane grinding to K for cylindrical grinding) are used.

Particular attention will be paid to effective cooling of the surface during grinding to prevent degradation of the material surface.

Electro-discharge machining

CROMIS ESR is also suitable for EDM machining (wire or electrode). Preferably, the machining will be carried out with a low current density and a high frequency in order to limit the thickness of the white layer as much as possible.

Then it is necessary to carry out a stress relieving at 25°C below the last tempering in order to reduce the level of residual stresses (which could lead to a risk of cracking) and to carry out a polishing to completely remove the white layer formed during the discharge machining process.

Welding

It is not recommended to weld CROMIS ESR but if this is mandatory it could be welded either in the annealed condition (better) or in the heat treated condition.

  • Method: TIG
  • Feeder wire: AISI 420
  • Preheating: 250°C. hold at 200°C during the welding operation
  • Post treatment:
    • In the treated state: tempering for a minimum of 2 hours at 20°C below the initial tempering temperature.
    • In the annealed state: carry out a soft annealing under the usual conditions: temperature: 840 – 870°C, duration 1h + 1h for 25 mm of thickness. slow cooling in the furnace (10 to 20°C/h).