Applications
Shafts, Gears, Aircraft Structural parts, Fittings, Fasteners, Valve parts
Features
- 15-5 PH is a martensitic precipitation-hardening stainless steel that offers excellent corrosion resistance, high strength, and good toughness. This alloy conforms to AMS 5659 and AMS 5862 and is commonly used in aerospace and power generation applications where the combination of high strength and corrosion resistance is essential.
- One of the benefits of 15-5 PH is that it is relatively easy to work with and can be readily machined, welded, and formed. However, to optimize the mechanical properties of this alloy, heat treatment may be necessary. The heat treatment process for 15-5 PH typically involves two steps: solution annealing and precipitation hardening.
- It can be produced either through consumable electrode melting (ESR) or Vacuum Arc Remelting (VAR). 15-5 PH stainless steel offers very good transverse properties and is corrosion resistant.
Standard
AMS 5659 / AMS 5862
Material
15-5 PH / UNS S15500 / W.Nr 1.4545
Chemical composition (Nominal) %
| Grade | C | Mn | Si | P | S | Cr |
|---|---|---|---|---|---|---|
| 15-5 PH | 0.07 max | 1.00 max | 1.00 max | 0.030 max | 0.015 max | 14.00-15.50 |
| Ni | Nb | Cu | Mo | Fe |
|---|---|---|---|---|
| 3.50-5.50 | 5xC%-0.45 | 2.50-4.50 | 0.50-max | Bal |
Physical properties
| Density | 7.8 g/cm3 |
|---|
Mechanical properties
| Condition | Specimen Orientation | Tensile Strength, min, MPa | Yield Strength, min. (0.2 % offset), min, MPa | Elongation in 2 in. or 50 mm (or 4D), % | Reduction of Area, min,% | Hardness, min, HB |
|---|---|---|---|---|---|---|
| H900 | L | 1310 | 1172 | 10 | 35 | 388 |
| T | 1310 | 1172 | 6 | 20 | ||
| H925 | L | 1172 | 1069 | 10 | 38 | 375 |
| T | 1172 | 1069 | 7 | 25 | ||
| H1025 | L | 1069 | 1000 | 12 | 45 | 331 |
| T | 1069 | 1000 | 8 | 32 | ||
| H1075 | L | 1000 | 862 | 13 | 45 | 311 |
| T | 1000 | 862 | 9 | 33 | ||
| H1100 | L | 965 | 793 | 14 | 45 | 302 |
| T | 965 | 793 | 10 | 34 | ||
| H1150 | L | 931 | 724 | 16 | 50 | 277 |
| T | 931 | 724 | 11 | 35 |
Round bar
Size range
| Product | Material | DIA Range | Length Range |
|---|---|---|---|
| ROUND BAR | 15-5 PH | Φ5mm ~ Φ500mm | 3000~6000mm |
Plate and sheet
Size range
| Product | Material | WD Range | Length Range | WT Range |
|---|---|---|---|---|
| PLATE & SHEET | 15-5 PH | 1000~2000mm | 2000~4000mm | 0.5~150mm |