Skip to main content

2379 PRIME

One of the most common cold work tool steel, with very good abrasive and adhesive wear resistance

2379 PRIME;

  • is a 12% Cr steel produced by a process that ensures a good level of cleanliness.
  • has a high abrasive wear resistant and also good adhesive wear resistance.
  • has a good dimensional stability, good compressive strength.
  • has a very good suitability for surface treatments such as gas, ionic or salt bath nitriding, as well as PVD or CVD coatings.

Applications

2379 PRIME is used for forming, blanking dies, deep drawing dies, shearing dies and tools and also in roll forming operations: rolls and tools.

2379 PRIME is also used for cold die and punches manufacturing, stone crushing balls, industrial knives and hand knives.

Main properties

  • Good abrasive and adhesive wear resistance
  • Good compressive strength
  • Good dimensional stability
  • Suitable for surface treatments

Chemical composition (typical)

C Mn Si P S Cr Mo V
1.52 0.50 0.35 ≤ 0.030 ≤ 0.025 12.0 0.85 0.85

Designation

Werkstoff Nr ISO China GB JIS Japan UK AISI USA Russia Gost AFNOR Other / Special
1,.2379 X153CrMoV12 -1 Cr12Mo1V1A SKD11 BD2 D2 – Z160CDV12 –

Structure

The structure of the 2379 PRIME is fine and homogeneous without precipitation or alignments of carbides.

The 2379 PRIME is ingot casted to guarantee fine primary carbides with a homogeneous distribution in the product.

Hardness at the time of delivery

Annealed for 255 HB max.

Physical properties

Temperature 20°C 100°C 200°C 300°C
Volumic mass kg/m³ 7700 7680 7650 7630
Young Modulus N/mm² 215000 205000 199000 193000
Thermal conductivity W/m.K 20 20 21 21.5
Coefficient of linear expansion 10-6/K 12 12.3 12.4 12.5

Heat treatment

Soft annealing

Temperature: 820 – 850°C, duration 1h + 1h for 25 mm thickness. slow cooling in the furnace (10 to 20°C/h). The atmosphere in the furnace must be reducing to avoid decarburization of the steel.

Stress relieving

After machining, it is recommended to perform stress relieving at 650°C for a minimum of 2 hours, followed by slow cooling in the furnace to 450°C.

Austenitization

In order to avoid any risk of cracking it is recommended to preheat in 2 steps.

  • 1st preheating step: temperature: 550°C time: 30 s/mm of thickness
  • 2nd preheating step: temperature: 850°C time: 30 s/mm of thickness

Recommended austenitizing temperature: 1030 – 1080°C. The holding time should not be too long to avoid a risk of grain coarsening and a loss of toughness. It is recommended to keep the part at the austenitizing temperature 30 minutes per inch of thickness as soon as the temperature of the surface reach the austenitization temperature.

Quenching medium

Oil at 80°C, vacuum (pressure > 6 bars), salt bath 500 – 550°C.
To ensure good toughness, treatment with oil or salt bath is preferable.

Sub zero treatment

For parts that need to have high dimensional stability and to increase wear resistance without reducing toughness, it is recommended to perform a subzero treatment at a temperature between -70°C and -190°C for 1 hour for 25 mm of thickness of the part.

The temperature range from -70°C up to -120°C (named cold treatment of steel) leads to the complete transformation of austenite into martensite and as a consequence to better stability associated with improved hardness and better wear resistance and the temperature range from -135°C down to -190°C (named cryotreatment of steel) leads also to the complete transformation of austenite and also the precipitation of ultrafine carbides improving a lot the wear resistance without modification of the toughness.

This treatment is optional for common applications.

Tempering

To ensure a minimum residual austenite rate as well as greater tool stability, it is essential to perform a double (triple is better) tempering. Each tempering is followed by a cooling under 100°C.

Each tempering time must be at least equal to 1h + 1h for 25 mm of thickness of the treated part (equivalent thermal thickness).

Hardness as a function of tempering temperature: The usual hardness for cold working uses is in the range of 58 to 61 HRC and is obtained by tempering between 450 and 500°C. Higher tempering temperature can be performed for hot work applications. In order to avoid the formation of large carbides that are detrimental to toughness, it is preferable to carry out austenitization at the lowest possible temperature, i.e. 1000 or 1020°C.

The table below shows the HRC hardness obtained as a function of the tempering temperature and the austenitization temperature.

Austenitisation temperature°C
Tempering temperature °C 1000 1025 1050 1080
100 60 61 62 –
200 59 60 60 –
300 58 58 58 58
400 57 58 59 57.5
450 57 58 60 59.5
500 57 60 61 61
550 54 55 55 56
600 44 45 47 50

2379 PRIME tempering curve: hardness (HRC) versus tempering temperature (°C) after austenitizing at 1000, 1025 and 1050 °C

Surface treatment

Nitriding

2379 PRIME can be nitrided at temperatures less than or equal to 20°C below tempering temperatures without risk of deterioration of the mechanical characteristics.

The hardness of the nitride layer is around 1100 HV1 and the thickness is dependent on the nitriding process.

PVD, CVD

2379 PRIME is suitable for all kinds of PVD and CVD treatment as soon as the treatment temperature is 30°C lower than the last tempering temperature.

Machining

The machining parameters below are given for information only and must be adapted according to the equipment and usual machining conditions.

Turning

Carbide tool
Rough machining
Carbide tool
Finishing
HSS tool
Finishing
Cutting speed m/min 100 – 150 140 – 200 10 – 15
Feed mm/r 0.2 – 0.4 0.1 – 0.2 0.1 – 0.3
Depth of cut mm 2 – 4 0.5 – 2 0.5 – 2

Milling: surfacing

Milling with carbide tools
Rough machining
Milling with carbide tools
½ Finishing
HSS tool
Finishing
Cutting speed m/min 100 – 120 160 – 180 80 -100
Feed mm/r 0.2 – 0.4 0.1 – 0.2 0.02 – 0.2
Depth of cut mm 2 – 4 0.5 – 2

Drilling: carbide drill

Carbide type Indexable insert Solid carbide Carbide tip
Cutting speed m/min 130 – 150 80 – 90 35 – 45
Feed mm/t 0.05 – 0.10 0.10 – 0.25 0.15 – 0.25

HSS twist drill

Drill diameter mm Cutting speed m/min Feed mm/t
< 5 10 – 12 0.05 – 0.15
5 – 10 10 – 12 0.15 – 0.20
10 – 15 10 – 12 0.20 – 0.25
15 – 20 10 – 12 0.25 – 0.30

Fine grinding

General indications for grinding wheels to be used on 2379 PRIME in the heat treated condition

Usually, rather soft vitrified aluminum oxide grinding wheels (grades G for plane grinding to K for cylindrical grinding) are used.

Particular attention will be paid to effective cooling of the surface during grinding to prevent degradation of the material surface.

Electro-discharge machining

2379 PRIME is also suitable for EDM machining (wire or electrode). Preferably, the machining will be carried out with a low current density and a high frequency in order to limit the thickness of the white layer as much as possible.

Then it is necessary to carry out a stress relieving at 25°C below the last tempering in order to reduce the level of residual stresses (which could lead to a risk of cracking) and to carry out a polishing to completely remove the white layer formed during the discharge machining process.

Welding

2379 PRIME cannot be welded.